Semi-coated super-hydrophobic quartz sand proppant and preparation method thereof

By forming a semi-coated hydrophobic layer and a network structure on the surface of quartz sand, the problems of insufficient hydrophobic properties and thermal stability of hydrophobic quartz sand proppant are solved, and efficient oil and gas extraction is achieved.

CN118995191AInactive Publication Date: 2024-11-22SHAANXI RUNBOXUAN CONSTRUCTION LABOR SERVICE CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411100781.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing hydrophobic quartz sand proppants have poor hydrophobic properties, poor thermal stability of hydrophobic layers, and complex preparation processes, which limits their application value in unconventional oil and gas reservoir development.

Method used

C14-C20 long-chain fatty acids are used to adsorb and dehydrate titanium dioxide to form a hydrophobic layer, which is then chemically bonded to the surface of quartz sand to form a semi-encapsulated structure. Epoxy resin is then used to cure the layer to form a network structure, thereby improving hydrophobicity and stability.

Benefits of technology

The prepared semi-coated superhydrophobic quartz sand proppant has excellent hydrophobicity and thermal stability, which can effectively reduce the cost of oil and gas extraction and increase oil and gas production. It is suitable for the extraction of unconventional oil and gas reservoirs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995191A_ABST
    Figure CN118995191A_ABST
Patent Text Reader

Abstract

The invention discloses a semi-coated super-hydrophobic quartz sand proppant and a preparation method thereof, and belongs to the technical field of oil and gas field fracturing proppants. The preparation method of the semi-coated super-hydrophobic quartz sand proppant comprises the following steps that in a first organic solvent, C14-C20 long-chain fatty acid serves as a modifier, titanium dioxide is added, the C14-C20 long-chain fatty acid and the titanium dioxide are subjected to adsorption and dehydration reactions, and titanium dioxide and long-chain fatty acid particles are prepared; acidizing quartz sand to obtain pretreated quartz sand; and in a second organic solvent, uniformly mixing the pretreated quartz sand with titanium dioxide and long-chain fatty acid particles, and carrying out chemical bond bonding reaction to prepare the super-hydrophobic quartz sand proppant. The preparation method comprises the following steps: uniformly mixing epoxy resin and a curing agent to obtain a mixed solution, adding super-hydrophobic quartz sand into the mixed solution, uniformly mixing, and curing to obtain the semi-coated super-hydrophobic quartz sand proppant.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of oil and gas field fracturing proppants, and in particular to a semi-coated super-hydrophobic quartz sand proppant and a preparation method thereof. Background Art

[0002] Fracturing technology is one of the important technologies for increasing the single well production and recovery rate of unconventional oil and gas reservoirs. Its core is that the fracturing fluid carries the proppant into the formation and fractures the formation to form a fracture network with sufficient length, sufficient width and certain conductivity, thereby providing a seepage channel for oil and gas extraction. In this technology, proppant has always been the key to the fracturing transformation effect and fracturing success rate. At present, quartz sand, ceramsite and coated proppant are still the three commonly used proppants in fracturing technology. Due to its advantages of low cost, high hardness, strong wear resistance and strong chemical stability, quartz sand is currently the most widely used fracturing proppant.

[0003] In recent years, the difficulty of exploration and development of unconventional natural oil and gas resources has increased significantly, while the demand for oil and gas production has increased significantly. This puts higher requirements on the performance of quartz sand proppants in fracturing technology. Therefore, the surface modification of quartz sand proppants has become a hot topic in oil and gas field production research. Studies have shown that hydrophobic quartz sand proppants can form water plugging and oil drainage channels in the fracture network generated by downhole fracturing. This is conducive to increasing oil and gas production while effectively reducing production costs. Therefore, hydrophobic quartz sand proppants have received more widespread attention.

[0004] However, the hydrophobic quartz sand proppant still has the following problems: first, the poor hydrophobic performance leads to poor water blocking performance of the seam network channel; second, the poor thermal stability of the hydrophobic layer on the quartz sand leads to poor stability of the water blocking and oil drainage channel; in addition, the complex preparation process leads to extremely high batch production costs. The above problems seriously restrict the practical application value of hydrophobic quartz sand proppant in unconventional oil and gas reservoir exploitation. Summary of the invention

[0005] In view of the above problems, the present invention provides a semi-coated super-hydrophobic quartz sand proppant and a preparation method thereof. The prepared semi-coated super-hydrophobic quartz sand proppant has high thermal stability and good hydrophobicity.

[0006] The first object of the present invention is to provide a method for preparing a semi-coated super-hydrophobic quartz sand proppant, comprising the following steps:

[0007] In the first organic solvent, C 14 -C 20 Long-chain fatty acids are used as modifiers, titanium dioxide is added, C 14 -C 20 Long-chain fatty acids react with titanium dioxide through adsorption and dehydration, and C14 -C 20 The long-chain fatty acids form a hydrophobic layer to prepare titanium dioxide@long-chain fatty acid particles;

[0008] Acidifying the quartz sand to obtain pretreated quartz sand;

[0009] In a second organic solvent, the pretreated quartz sand and the titanium dioxide @ long-chain fatty acid particles are uniformly mixed to produce a chemical bond reaction, and the titanium dioxide @ long-chain fatty acid particles are wrapped on the surface of the quartz sand to provide hydrophobic groups and a rough structure, thereby preparing a super-hydrophobic quartz sand proppant;

[0010] The epoxy resin and the curing agent are mixed evenly to obtain a mixed liquid, and super-hydrophobic quartz sand is added to the mixed liquid and mixed evenly. The epoxy resin forms a network structure during the curing process and serves as a filler to fill defects and pores. After the curing is completed, a semi-coated super-hydrophobic quartz sand proppant is prepared.

[0011] In one embodiment of the present invention, C 14 -C 20 The long-chain fatty acid is one of myristic acid, palmitic acid, pearlitic acid, stearic acid and arachidic acid.

[0012] In one embodiment of the present invention, C 14 -C 20 The ratio of long-chain fatty acid, titanium dioxide and first organic solvent is 6g-18g:4g-12g:20mL-100mL. 14 -C 20 The ratio of long-chain fatty acid, titanium dioxide and the first organic solvent is 6g:4g:20mL, 6g:5g:30mL, 6g:6g:40mL, 6g:7g:50mL, 6g:8g:60mL, 6g:9g:70mL, 6g:9g:80mL, 6g:10g:90mL, 6g:11g:100mL, 6g:12g:100mL, 8g:4g:20mL, 10g:4g:20mL, 12g:4g:20mL, etc.; but it is not limited to the listed values, other values ​​not listed within the above numerical range are also applicable, so they will not be repeated here.

[0013] In one embodiment of the present invention, the reaction temperature of the adsorption and dehydration reaction is 25°C to 65°C, and the reaction time is 4h to 8h. For example, the reaction temperature of the adsorption and dehydration reaction is 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, etc.; the reaction time is 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h, 8h, etc.; but it is not limited to the listed values, and other values ​​not listed in the above numerical range are also applicable, so they will not be repeated here.

[0014] In one embodiment of the present invention, the acidification treatment is carried out by immersion treatment with a hydrochloric acid solution for 20 minutes to 60 minutes, and the mass concentration of hydrochloric acid in the hydrochloric acid solution is 5.0% to 40%. For example, the immersion treatment is 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, 45 minutes, 50 minutes, 55 minutes, 60 minutes, etc.; the mass concentration of hydrochloric acid in the hydrochloric acid solution is 5.0%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, etc.; but it is not limited to the listed values, and other values ​​not listed in the above numerical range are also applicable, so they will not be repeated here.

[0015] In one embodiment of the present invention, the ratio of pretreated quartz sand, titanium dioxide @ long-chain fatty acid particles and the second organic solvent is 2g to 6g: 0.4g to 1.2g: 20mL. For example, the ratio of pretreated quartz sand, titanium dioxide @ long-chain fatty acid particles and the second organic solvent is 2g: 0.4g: 20mL, 2g: 0.6g: 20mL, 2g: 0.8g: 20mL, 2g: 1.0g: 20mL, 2g: 1.2g: 20mL, 4g: 0.4g: 20mL, 6g: 0.4g: 20mL, etc.; but it is not limited to the listed values, and other values ​​not listed in the above numerical range are also applicable, so they will not be repeated here.

[0016] In one embodiment of the present invention, the reaction temperature of the chemical bonding reaction is 70°C to 90°C, and the reaction time is 7h to 11h. For example, the reaction temperature of the chemical bonding reaction is 70°C, 75°C, 80°C, 85°C, 90°C, etc., and the reaction time is 7h, 8h, 9h, 10h, 11h, etc. However, it is not limited to the listed values, and other values ​​not listed in the above numerical range are also applicable, so they will not be repeated here.

[0017] In one embodiment of the present invention, the molar ratio of the epoxy resin to the curing agent is 1 to 4:1, for example, the molar ratio of the epoxy resin to the curing agent is 1:1, 2:1, 3:1, 4:1, etc.;

[0018] The mass ratio of the mixed liquid to the super-hydrophobic quartz sand is 0.1:0.5 to 3.5. For example, the mass ratio of the mixed liquid to the super-hydrophobic quartz sand is 0.1:0.5, 0.1:1, 0.1:1.5, 0.1:2, 0.1:2.5, 0.1:3, 0.1:3.5, etc. However, it is not limited to the listed values, and other values ​​not listed in the above numerical range are also applicable, which will not be repeated here.

[0019] In one embodiment of the present invention, the curing temperature is 100°C to 150°C, and the curing time is 2h to 7h. For example, the curing temperature is 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, etc., and the curing time is 2h, 3h, 4h, 5h, 6h, 7h, etc. However, it is not limited to the listed values, and other values ​​not listed in the above numerical range are also applicable, which will not be repeated here.

[0020] The second object of the present invention is to provide a semi-coated super-hydrophobic quartz sand proppant prepared by the above preparation method.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] (1) The present invention provides a semi-coated super-hydrophobic quartz sand proppant, firstly with C 14 -C 20 Long-chain fatty acids are used as modifiers and are physically adsorbed by titanium dioxide, as well as C 14 -C 20 The carboxyl groups in the long-chain fatty acids and the hydroxyl groups in the titanium dioxide undergo a dehydration reaction, completing the modification of the titanium dioxide to obtain titanium dioxide@long-chain fatty acid particles; the addition of long-chain fatty acids can form a dense hydrophobic layer on the surface of the quartz sand, effectively blocking the penetration of water molecules and enhancing the hydrophobic properties of the material; further, the quartz sand and the titanium dioxide@long-chain fatty acid particles are hydrogen bonded and polycondensed with hydroxyl groups to coat the titanium dioxide@long-chain fatty acid particles on the surface of the quartz sand, thereby providing hydrophobic groups and forming a rough structure, and finally a continuous network structure can be formed during the curing process of the epoxy resin, which can effectively transfer and disperse stress, while also filling tiny defects and pores on the surface of the hydrophobic layer, further improving the stability of the material.

[0023] (2) The raw materials of the semi-coated super-hydrophobic proppant of the present invention are easy to obtain, have a wide source, and are low in cost.

[0024] (3) The preparation process of the present invention is simple and can be mass-produced.

[0025] (4) The semi-coated super-hydrophobic proppant prepared by the present invention has excellent super-hydrophobicity and thermal stability, which can effectively reduce the cost of oil and gas production, increase oil and gas production, and meet the requirements of unconventional oil and gas reservoir production. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1The super depth of field images and SEM images of the original quartz sand proppant and the proppant prepared in Example 4 and Comparative Example 1. Among them, (a1) and (a2) are the super depth of field images and SEM images of the original quartz sand proppant, (b1) and (b2) are the super depth of field images and SEM images of the titanium dioxide@stearic acid modified super hydrophobic quartz sand proppant prepared in Example 4, (c1) and (c2) are the super depth of field images and SEM images of the semi-coated super hydrophobic quartz sand proppant prepared in Example 4.

[0027] Figure 2 The contact angle test results of the original quartz sand proppant and the proppant prepared in Example 4 and Comparative Example 1 are shown. Among them, (a) is the contact angle of the original quartz sand proppant, (b) is the contact angle of the titanium dioxide@stearic acid modified superhydrophobic quartz sand proppant prepared in Comparative Example 1, and (c) is the contact angle of the semi-coated superhydrophobic quartz sand proppant prepared in Example 4.

[0028] Figure 3 These are the test results of the crushing rate of the original quartz sand proppant and the proppant prepared in Example 4 and Comparative Example 1.

[0029] Figure 4 The TGA graphs of the original quartz sand proppant and the proppant prepared in Example 4 and Comparative Examples 1-2 are shown. DETAILED DESCRIPTION

[0030] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] As shown in the background technology, the existing hydrophobic quartz sand proppant has the problems of poor hydrophobic performance and poor thermal stability of the hydrophobic layer. Based on this, the present invention provides a method for preparing a semi-coated super-hydrophobic quartz sand proppant. The specific technical scheme is as follows.

[0032] In the first organic solvent, C 14 -C 20 Long-chain fatty acids are used as modifiers. When titanium dioxide is added, on the one hand, the two are combined with each other through physical adsorption. On the other hand, the carboxyl groups in the long-chain fatty acids react with the hydroxyl groups on the surface of titanium dioxide to combine with each other through dehydration reaction, and C 14 -C 20 The long-chain fatty acids form a hydrophobic layer, and finally titanium dioxide@long-chain fatty acid particles are prepared;

[0033] Acidizing the quartz sand to remove impurities such as yellow skin, water rust and organic chromosomes on the surface of the quartz sand, improve its surface properties, increase the purity and surface smoothness of the quartz sand, and prepare pretreated quartz sand;

[0034] In the second organic solvent, the pretreated quartz sand and the titanium dioxide @ long-chain fatty acid particles are chemically bonded to prepare a super-hydrophobic quartz sand proppant. Specifically, there are hydroxyl groups on the surface of both titanium dioxide and quartz sand. On the one hand, these hydroxyl groups are mutually adsorbed through hydrogen bonds to achieve surface bonding; on the other hand, the hydroxyl groups between the two react through polycondensation to coat the surface of the quartz sand with a layer of nano-titanium dioxide, achieving chemical coating, and finally forming modified quartz sand with stable chemical properties.

[0035] After the epoxy resin and the curing agent are mixed evenly to obtain a mixed solution, super-hydrophobic quartz sand is added to the mixed solution and mixed evenly, the epoxy resin forms a network structure during the curing process and fills defects and pores as a filler, and after the curing is completed, a semi-coated super-hydrophobic quartz sand proppant is prepared. After the super-hydrophobic quartz sand proppant is coated and modified with epoxy resin, the stability and mechanical properties of the proppant can be further improved, so that the proppant can be used for a long time in a complex environment.

[0036] In order to better improve the hydrophobic properties of the material, the present invention selects long-chain fatty acids as modifiers. This is because long-chain fatty acids have longer carbon chains and can form a denser and more stable hydrophobic layer on the surface of the material. This long-chain structure allows the fatty acid molecules to better cover the surface of the material, reducing the contact between water molecules and the surface of the material, thereby improving the hydrophobic properties of the material. And as the number of carbon atoms increases, the length and hydrophobicity of the fatty acid molecules will increase. Therefore, the present invention selects long-chain fatty acids with a carbon number greater than 14 to obtain a better hydrophobic effect. The longer carbon chain makes the hydrophobic layer formed by the fatty acid molecules on the surface of the material more stable and not easily destroyed or fallen off. Further, the C used in the present invention 14 -C 20 The long-chain fatty acid is one of myristic acid, palmitic acid, pearlitic acid, stearic acid, and arachidic acid.

[0037] In some preferred embodiments, after the quartz sand is added to a mixed solution of water and ethanol for ultrasonic cleaning, it is immersed in a hydrochloric acid solution for acidification to obtain pretreated quartz sand. During the ultrasonic cleaning process, the ratio of quartz sand to the mixed solution is 4g-12g:30mL-100mL, the volume ratio of water to ethanol in the mixed solution is 1:0.5-4, and the ultrasonic time is 20min.

[0038] In some preferred embodiments, the molar ratio of epoxy resin to curing agent is 1-4:1, and the mass ratio of the mixed solution to super-hydrophobic quartz sand is 0.1:0.5-3.5.

[0039] Specifically, the mixed solution and super-hydrophobic quartz sand are stirred at 25-90° C. for 0.5 h to 2.5 h, and finally the product is placed in an oven at 100° C. to 150° C. for drying for 2 h to 7 h, and the solidified sample is taken out and ground into powder to obtain the final product.

[0040] The semi-coated super-hydrophobic quartz sand proppant prepared by the present invention has excellent super-hydrophobicity, thermal stability and mechanical properties, can be used in hydraulic fracturing technology, and forms efficient water-blocking passages in downhole fracture networks, thereby effectively reducing oil and gas production costs and increasing oil and gas production, and has broad application prospects in unconventional oil and gas production.

[0041] The following experimental methods and detection methods are conventional methods unless otherwise specified; the following reagents and raw materials are commercially available unless otherwise specified, and the present invention does not make any special restrictions hereon. It should be noted that the TiO2 used in the present invention is anatase TiO2, because it has a high surface hydroxyl content, is more likely to chemically react or physically adsorb with long-chain fatty acids, and is more likely to achieve effective surface modification.

[0042] Example 1

[0043] (1) 4.0 g of 30 nm anatase TiO2 and 16.0 g of myristic acid were added to 100 mL of ethanol solution, magnetically stirred at 65 ° C and a stirring rate of 150 rpm for 8 h, then centrifuged and dried in an oven at 50 ° C for 18 h to obtain titanium dioxide @ myristic acid;

[0044] (2) adding 4.0 g of 120 mesh quartz sand to 100 mL of a mixed solution of distilled water and ethanol in a volume ratio of 1:4, and ultrasonically cleaning for 20 min, placing the preliminarily cleaned quartz sand in a hydrochloric acid solution, wherein the mass content of hydrochloric acid is 5.0 wt%, and then soaking for 60 min, washing with distilled water and the pH value of the distilled water after washing is 7, drying at 50 ° C, drying for 18 h, and obtaining pretreated quartz sand after drying;

[0045] (3) Weigh 2.0 g of the pretreated quartz sand in step (2) and 0.4 g of the titanium dioxide @ myristic acid particles in step (1) and add them to 20 mL of ethanol solution, first ultrasonically treat for 50 min, then magnetically stir at 90 ° C and a stirring rate of 150 rpm for 7 h, and then put it into an oven at 70 ° C for 16 h to obtain a titanium dioxide @ myristic acid modified superhydrophobic quartz sand proppant.

[0046] (4) Weigh 5.0 g of epoxy resin 862 and 5.3 g of curing agent diethyltoluenediamine respectively, mix them evenly, and mechanically stir them at 25° C. and a stirring rate of 500 rpm for 2.5 h to obtain a mixed solution. Then weigh 0.1 g of the mixed solution and 3.0 g of the superhydrophobic quartz sand proppant in the above step (3), mix them evenly, and put them into an oven at 150° C. for 2 h to obtain a semi-coated superhydrophobic quartz sand proppant.

[0047] Example 2

[0048] (1) 6.0 g of 40 nm anatase TiO2 and 18.0 g of palmitic acid were added to 80 mL of ethanol solution, magnetically stirred at 55 ° C and a stirring rate of 200 rpm for 7 h, then centrifuged and dried in an oven at 60 ° C for 16 h to obtain titanium dioxide @ palmitic acid;

[0049] (2) 6.0 g of 100-mesh quartz sand was added to 80 mL of a mixed solution of distilled water and ethanol in a volume ratio of 1:3, and ultrasonically cleaned for 20 min. The quartz sand after preliminary cleaning was placed in a hydrochloric acid solution, wherein the mass content of hydrochloric acid was 10.0 wt%, and then soaked for 50 min. The quartz sand was washed with distilled water and the pH value of the distilled water after washing was 7. The drying temperature was 60 ° C. and the drying time was 16 h. After drying, pretreated quartz sand was obtained;

[0050] (3) Weigh 3.0 g of the pretreated quartz sand in step (2) and 0.6 g of the titanium dioxide @ palmitic acid particles in step (1) and add them to 20 mL of ethanol solution, first ultrasonically treat for 40 min, then magnetically stir at 85 ° C and a stirring rate of 200 rpm for 8 h, and then put it into an oven at 80 ° C for 14 h to obtain a titanium dioxide @ palmitic acid modified superhydrophobic quartz sand proppant.

[0051] (4) Weigh 5.0 g of epoxy resin 862 and 2.6 g of curing agent diethyltoluenediamine respectively, mix them evenly, and mechanically stir them at 40° C. and a stirring rate of 400 rpm for 2.0 h to obtain a mixed solution. Then weigh 0.1 g of the mixed solution and 2.0 g of the superhydrophobic quartz sand proppant in the above step (3), mix them evenly, and put them into an oven at 140° C. and dry them for 3 h to obtain a semi-coated superhydrophobic quartz sand proppant.

[0052] Example 3

[0053] (1) 8.0 g of 50 nm anatase TiO2 and 16.0 g of pearlescent fatty acid were added to 60 mL of ethanol solution, magnetically stirred at 45 ° C and a stirring rate of 250 rpm for 6 h, then centrifuged and dried in an oven at 70 ° C for 4 h to obtain titanium dioxide @ pearlescent fatty acid;

[0054] (2) 8.0 g of 80-mesh quartz sand was added to 60 mL of a mixed solution of distilled water and ethanol in a volume ratio of 1:2, and ultrasonically cleaned for 20 min. The quartz sand after preliminary cleaning was placed in a hydrochloric acid solution, wherein the mass content of hydrochloric acid was 20.0 wt %, and then soaked for 40 min. The quartz sand was washed with distilled water and the pH value of the distilled water after washing was 7. The drying temperature was 70° C. and the drying time was 14 h. After drying, pretreated quartz sand was obtained;

[0055] (3) Weigh 4.0 g of the pretreated quartz sand in step (2) and 0.8 g of the titanium dioxide @ pearlescent fatty acid particles in step (1) and add them to 20 mL of ethanol solution, first ultrasonically treat for 30 min, then magnetically stir at 80 ° C and a stirring rate of 250 rpm for 9 h, and then put it into an oven at 90 ° C for 12 h to obtain a titanium dioxide @ pearlescent fatty acid modified superhydrophobic quartz sand proppant.

[0056] (4) Weigh 5.0 g of epoxy resin 862 and 1.8 g of curing agent diethyltoluenediamine respectively and mix them evenly, and mechanically stir them at 60° C. and a stirring rate of 300 rpm for 1.0 h to obtain a mixed solution, then weigh 0.1 g of the mixed solution and 1.0 g of the superhydrophobic quartz sand proppant in the above step (3), mix them evenly, and then put them into an oven at 130° C. and dry them for 4 h to obtain a semi-coated superhydrophobic quartz sand proppant.

[0057] Example 4

[0058] (1) 10.0 g of 60 nm anatase TiO2 and 10.0 g of stearic acid were added to 40 mL of ethanol solution, magnetically stirred at 35° C. and 300 rpm for 5 h, then centrifuged and dried in an oven at 80° C. for 12 h to obtain titanium dioxide @ stearic acid;

[0059] (2) adding 10.0 g of 60-mesh quartz sand to 40 mL of a mixed solution of distilled water and ethanol in a volume ratio of 1:1, ultrasonically cleaning for 20 min, placing the preliminarily cleaned quartz sand in a hydrochloric acid solution, wherein the mass content of hydrochloric acid is 30.0 wt %, then soaking for 30 min, washing with distilled water and the pH value of the distilled water after washing is 7, drying at 80 ° C, drying for 12 h, and obtaining pretreated quartz sand after drying;

[0060] (3) Weigh 5.0 g of the pretreated quartz sand in step (2) and 1.0 g of the titanium dioxide @ stearic acid particles in step (1) and add them to 20 mL of ethanol solution, first ultrasonically treat for 20 min, then magnetically stir at 75 ° C and a stirring rate of 300 rpm for 10 h, and then put it into an oven at 100 ° C for 10 h to obtain a titanium dioxide @ stearic acid modified superhydrophobic quartz sand proppant.

[0061] (4) Weigh 5.0 g of epoxy resin 862 and 1.3 g of curing agent diethyltoluenediamine respectively, mix them evenly, and mechanically stir them at 80° C. and a stirring rate of 200 rpm for 0.5 h to obtain a mixed solution. Then weigh 0.1 g of the mixed solution and 0.75 g of the super-hydrophobic quartz sand proppant in the above step (3), mix them evenly, and put them in an oven at 120° C. to dry for 5 h to obtain a semi-coated super-hydrophobic quartz sand proppant.

[0062] Example 5

[0063] (1) 12.0 g of 70 nm anatase TiO2 and 6.0 g of arachidic acid were added to 20 mL of ethanol solution, magnetically stirred at 25 ° C and 350 rpm for 4 h, then centrifuged and dried in an oven at 90 ° C for 10 h to obtain titanium dioxide @ arachidic acid;

[0064] (2) adding 12.0 g of 40-mesh quartz sand to 30 mL of a mixed solution of distilled water and ethanol in a volume ratio of 1:2, ultrasonically cleaning for 20 min, placing the preliminarily cleaned quartz sand in a hydrochloric acid solution, wherein the mass content of hydrochloric acid is 40.0 wt%, then soaking for 20 min, washing with distilled water and the pH value of the distilled water after washing is 7, drying at 90 ° C, drying for 10 h, and obtaining pretreated quartz sand after drying;

[0065] (3) Weigh 6.0 g of the pretreated quartz sand in step (2) and 1.2 g of the titanium dioxide @ arachidic acid particles in step (1) and add them to 20 mL of ethanol solution, first ultrasonically treat for 10 min, then magnetically stir at 70 ° C and a stirring rate of 350 rpm for 11 h, and then put into an oven at 110 ° C for 8 h to obtain a titanium dioxide @ arachidic acid modified superhydrophobic quartz sand proppant.

[0066] (4) Weigh 5.0 g of epoxy resin 862 and 1.1 g of curing agent diethyltoluenediamine respectively, mix them evenly, and mechanically stir them at 90° C. and a stirring rate of 100 rpm for 0.5 h to obtain a mixed solution. Then weigh 0.1 g of the mixed solution and 0.5 g of the super-hydrophobic quartz sand proppant in the above step (3), mix them evenly, and then put them into an oven at 110° C. and dry them for 7 h to obtain a semi-coated super-hydrophobic quartz sand proppant.

[0067] Comparative Example 1

[0068] (1) 10.0 g of 60 nm anatase TiO2 and 10.0 g of stearic acid were added to 40 mL of ethanol solution, magnetically stirred at 35° C. and 300 rpm for 5 h, then centrifuged and dried in an oven at 80° C. for 12 h to obtain titanium dioxide @ stearic acid;

[0069] (2) adding 10.0 g of 60-mesh quartz sand to 40 mL of a mixed solution of distilled water and ethanol in a volume ratio of 1:1, ultrasonically cleaning for 20 min, placing the preliminarily cleaned quartz sand in a hydrochloric acid solution, wherein the mass content of hydrochloric acid is 30.0 wt %, then soaking for 30 min, washing with distilled water and the pH value of the distilled water after washing is 7, drying at 80 ° C, drying for 12 h, and obtaining pretreated quartz sand after drying;

[0070] (3) Weigh 5.0 g of the pretreated quartz sand in step (2) and 1.0 g of the titanium dioxide @ stearic acid particles in step (1) and add them to 20 mL of ethanol solution, first ultrasonically treat for 20 min, then magnetically stir at 75 ° C and a stirring rate of 300 rpm for 10 h, and then put it into an oven at 100 ° C for 10 h to obtain a titanium dioxide @ stearic acid modified superhydrophobic quartz sand proppant.

[0071] Comparative Example 2

[0072] (1) 10.0 g of 60-mesh quartz sand was added to 40 mL of a mixed solution of distilled water and ethanol in a volume ratio of 1:1, and ultrasonically cleaned for 20 min. The quartz sand after preliminary cleaning was placed in a hydrochloric acid solution, wherein the mass content of hydrochloric acid was 30.0 wt %, and then soaked for 30 min. The quartz sand was washed with distilled water and the pH value of the distilled water after washing was 7. The drying temperature was 80° C. and the drying time was 12 h. After drying, pretreated quartz sand was obtained;

[0073] (2) Weigh 5.0 g of epoxy resin 862 and 1.3 g of curing agent diethyltoluenediamine respectively, mix them evenly, and mechanically stir them at 80° C. and a stirring rate of 200 rpm for 0.5 h to obtain a mixed solution. Then weigh 0.1 g of the mixed solution and 0.75 g of the pretreated quartz sand in the above step (3), mix them evenly, and put them into an oven at 120° C. for 5 h to obtain semi-coated original quartz sand.

[0074] The semi-coated superhydrophobic quartz sand proppants prepared in Examples 1 to 5 all have good superhydrophobicity, thermal stability and mechanical properties, which are illustrated below by the semi-coated superhydrophobic quartz sand proppant prepared in Example 4, the titanium dioxide@stearic acid modified superhydrophobic quartz sand proppant prepared in Comparative Example 1, and the original quartz sand proppant.

[0075] Figure 1The super depth of field images and SEM images of the original quartz sand proppant and the proppant prepared in Example 4 and Comparative Example 1. Among them, Figures (a1) and (a2) are the super depth of field images and SEM images of the original quartz sand proppant, Figures (b1) and (b2) are the super depth of field images and SEM images of the super hydrophobic quartz sand proppant modified by titanium dioxide @ stearic acid prepared in Comparative Example 1, and Figures (c1) and (c2) are the super depth of field images and SEM images of the semi-coated super hydrophobic quartz sand proppant prepared in Example 4. It can be seen from Figures (a1) and (a2) that the surface of the original quartz sand is smooth and flat, and no other small particles exist. It can be seen from Figures (b1) and (b2) that the surface of the modified quartz sand proppant has no obvious edges and corners, and there are a large number of fine particles on the surface. Under the action of the modifier, the super hydrophobic quartz sand proppant modified by titanium dioxide @ stearic acid has no obvious agglomeration phenomenon, is more evenly distributed, has improved dispersibility, and has a good effect. Figures (c1) and (c2) show that in addition to some nanoparticles, there are also parts coated by epoxy resin on the surface of quartz sand, but there are also areas that are not coated by epoxy resin, thus achieving semi-coating of quartz sand by epoxy resin.

[0076] Figure 2 The contact angle test results of the original quartz sand proppant and the proppant prepared in Example 4 and Comparative Example 1. Among them, Figure (a) is the contact angle of the original quartz sand proppant, Figure (b) is the contact angle of the super-hydrophobic quartz sand proppant modified with titanium dioxide @ stearic acid prepared in Comparative Example 1, and Figure (c) is the contact angle of the semi-coated super-hydrophobic quartz sand proppant prepared in Example 4. It can be seen from Figure (a) that the water contact angle of the original quartz sand is only 18.1°, which is not hydrophobic. This is because the surface of the original quartz sand is smooth and flat, and does not have hydrophobic functional groups. Figure (b) can be seen that the water contact angle of the quartz sand proppant modified with titanium dioxide @ stearic acid reaches 157.9°, which has good super-hydrophobicity, because the surface of the quartz sand is combined with nanoparticles, providing a rough structure and hydrophobic groups. Figure (c) can be seen that the water contact angle of the semi-coated super-hydrophobic quartz sand proppant reaches 152.6°, which still has super-hydrophobicity.

[0077] Figure 3 The crushing rate test results of the original quartz sand proppant and the proppant prepared in Example 4 and Comparative Example 1 are shown. The crushing rates of the original quartz sand proppant, the super-hydrophobic quartz sand proppant modified with titanium dioxide @ stearic acid and the semi-coated super-hydrophobic quartz sand proppant are 2.07%, 1.58% and 1.31%, respectively, which have met the use requirements of the proppant, but the super-hydrophobic quartz sand proppant semi-coated with epoxy resin has the lowest crushing rate and has better mechanical properties.

[0078] Figure 4TGA graphs of the original quartz sand proppant and the proppant prepared in Example 4 and Comparative Examples 1 to 2 are provided to further analyze the thermal stability. For the original quartz sand proppant, there is no weight loss within the temperature range, and the final weight residue is about 99%. This slight weight loss is due to the removal of moisture on the surface of the original quartz sand proppant. For the treated quartz sand proppant, the main weight loss stage is 146°C to 280°C, which may be due to the thermal degradation of fatty acids on the TiO2 surface. The superhydrophobic quartz sand prepared in Comparative Example 1, the semi-coated original proppant prepared in Comparative Example 2, and the semi-coated superhydrophobic quartz sand proppant prepared in Example 4 began to lose mass at 146°C, 224°C, and 237°C, respectively. As the temperature further increased from 280°C to 800°C, a very slight weight loss was observed, which may be the result of fatty acid degradation. At 800℃, the weight loss residual rate of the modified proppant is 95.66%, the weight loss residual rate of the semi-coated original proppant is 88.87%, and the weight loss residual rate of the semi-coated super-hydrophobic quartz sand proppant is 82.44%. Therefore, the semi-coated super-hydrophobic quartz sand proppant has better thermal stability. Excellent thermal stability can improve the stability of the water plugging and oil drainage channels.

[0079] The semi-coated super-hydrophobic quartz sand proppant provided by the present invention can effectively reduce the attachment of water molecules on the proppant surface due to its surface hydrophobic properties, thereby alleviating or eliminating the water lock effect, and helping to keep the oil and gas channels unobstructed. In addition, the droplet rolling ability of the proppant surface is very strong, which can naturally repel and remove dirt and impurities on the surface, reducing the blockage problem caused by impurity accumulation. Therefore, the semi-coated super-hydrophobic quartz sand proppant can significantly increase the production and recovery rate of oil and gas wells, and bring greater economic benefits to the development of oil and gas fields.

[0080] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0081] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a semi-coated super-hydrophobic quartz sand proppant, characterized in that: The following steps are involved: In the first organic solvent, C 14 -C 20 Long-chain fatty acids are used as modifiers, titanium dioxide is added, C 14 -C 20 Long-chain fatty acids react with titanium dioxide through adsorption and dehydration, and C 14 -C 20 The long-chain fatty acids form a hydrophobic layer to prepare titanium dioxide@long-chain fatty acid particles; Acidifying the quartz sand to obtain pretreated quartz sand; In a second organic solvent, the pretreated quartz sand and the titanium dioxide @ long-chain fatty acid particles are uniformly mixed to produce a chemical bond reaction, and the titanium dioxide @ long-chain fatty acid particles are wrapped on the surface of the quartz sand to provide hydrophobic groups and a rough structure, thereby preparing a super-hydrophobic quartz sand proppant; The epoxy resin and the curing agent are mixed evenly to obtain a mixed liquid, and super-hydrophobic quartz sand is added to the mixed liquid and mixed evenly. The epoxy resin forms a network structure during the curing process and serves as a filler to fill defects and pores. After the curing is completed, a semi-coated super-hydrophobic quartz sand proppant is prepared.

2. The method for preparing a semi-coated super-hydrophobic quartz sand proppant according to claim 1, characterized in that: C 14 -C 20 The long-chain fatty acid is one of myristic acid, palmitic acid, pearlitic acid, stearic acid and arachidic acid.

3. The method for preparing a semi-coated super-hydrophobic quartz sand proppant according to claim 1, characterized in that: C 14 -C 20 The ratio of the long-chain fatty acid, titanium dioxide and the first organic solvent is 6 g to 18 g: 4 g to 12 g: 20 mL to 100 mL.

4. The method for preparing a semi-coated super-hydrophobic quartz sand proppant according to claim 1, characterized in that: The reaction temperature of the adsorption and dehydration reaction is 25°C to 65°C, and the reaction time is 4h to 8h.

5. The method for preparing a semi-coated super-hydrophobic quartz sand proppant according to claim 1, characterized in that: The acidification treatment is carried out by immersing in a hydrochloric acid solution for 20 minutes to 60 minutes, and the mass concentration of the hydrochloric acid in the hydrochloric acid solution is 5.0% to 40%.

6. The method for preparing a semi-coated super-hydrophobic quartz sand proppant according to claim 1, characterized in that: The ratio of pretreated quartz sand, titanium dioxide @ long-chain fatty acid particles and the second organic solvent is 2g-6g:0.4g-1.2g:20mL.

7. The method for preparing a semi-coated super-hydrophobic quartz sand proppant according to claim 1, characterized in that: The reaction temperature of the chemical bond reaction is 70°C to 90°C, and the reaction time is 7h to 11h.

8. The method for preparing a semi-coated super-hydrophobic quartz sand proppant according to claim 1, characterized in that: The molar ratio of the epoxy resin to the curing agent is 1-4:1, and the mass ratio of the mixed liquid to the super-hydrophobic quartz sand is 0.1:0.5-3.

5.

9. The method for preparing a semi-coated super-hydrophobic quartz sand proppant according to claim 1, characterized in that: The curing temperature is 100°C ~ 150°C, and the curing time is 2°C ~ 7h.

10. A semi-coated super-hydrophobic quartz sand proppant prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Environment-friendly biodegradable waterproof coiled material and preparation method thereof

    CN119610800A

  • Environment-friendly biodegradable waterproofing membrane and preparation method thereof

    CN119610800B

  • Hydrophobic petroleum fracturing propping agent and preparation method thereof

    CN120775578A