Degradable high-carbon steel stretching liquid

By using a combination scheme of modified oleate, anti-rust agent and extreme pressure anti-wear agent in high-carbon steel processing, a degradable high-carbon steel stretching liquid was prepared, which solved the problem of traditional stretching oil in high-carbon steel The problems of insufficient lubrication performance and non-degradable in carbon steel processing have achieved high lubricity, rust resistance and wear resistance, and improved processing efficiency and product quality.

CN118995305APending Publication Date: 2024-11-22AN HUI TECHSEA CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411054131.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Traditional stretching oils have problems such as insufficient lubricating performance, flammable, harmful components, difficulty in cleaning, and lack of degradability in high-carbon steel processing, which limits its application areas.

Method used

Using a compounding scheme of 38-68% modified oleate, 1-3% anti-rust agent, 3-10% extreme pressure anti-wear agent, 0.1-1% anti-hard water agent, and 10-20% surfactant, through A specific process step prepares a degradable high-carbon steel stretch liquid, including the use of tetrasodium ethylenediaminetetraacetate and ether carboxylic acid as anti-hardening water agents, W/O and O/W surfactants When used, the extremely pressure antiwear agent produced contains phosphorus, sulfur and nitrogen elements to enhance antiwear properties.

Benefits of technology

The produced stretching liquid has excellent anti-rust effect, high lubricity, degradability and extreme pressure wear resistance, which can effectively improve the woven and cracking phenomena in high-carbon steel processing, and improve processing efficiency and product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004975818220000031
    Figure BDA0004975818220000031
  • Figure BDA0004975818220000032
    Figure BDA0004975818220000032
  • Figure BDA0004975818220000091
    Figure BDA0004975818220000091
Patent Text Reader

Abstract

The invention discloses degradable high-carbon steel stretching liquid, and belongs to the technical field of metal forming machining. Comprising the following raw materials in percentage by mass: 38-68% of modified oleate, 1-3% of an anti-rust agent, 3-10% of an anti-wear reagent at extreme pressure, 0.1-1% of a hard water resistant agent, 10-20% of a surfactant and the balance of water. The prepared antirust agent has an excellent antirust effect on high-carbon steel; the prepared modified oleate has high lubricating property relative to oleic acid; compared with mineral oil in the traditional stretching liquid, the stretching liquid provided by the invention has degradability; the prepared extreme pressure anti-wear agent contains three elements of phosphorus, sulfur and nitrogen, can play a synergistic role, greatly enhances the extreme pressure anti-wear performance of the stretching liquid, and also can improve the galling and cracking phenomena of a workpiece treated by the stretching liquid; therefore, the prepared drawing liquid is good in antirust effect, has high lubricity, degradability and extreme pressure antiwear property, can improve the galling and cracking phenomena, and has important application value in the technical field of metal forming processing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal forming processing, and in particular relates to a degradable high-carbon steel drawing liquid. Background Art

[0002] High carbon steel is a kind of steel with high carbon content. After proper heat treatment or cold drawing hardening, it has high strength and hardness, as well as high elastic limit and fatigue limit. However, due to the high hardness and high carbon content of high carbon steel, it has high requirements for lubrication performance during processing, especially during stretching, to avoid scratches, deformation and cracking during processing.

[0003] Drawing oil is a metalworking oil specially used for metal drawing and stamping. It can provide the required lubrication performance, reduce friction and wear during processing, thereby improving processing efficiency and product quality. It is widely used in difficult-to-process metals such as high-carbon steel.

[0004] Traditional stretching oils mainly include mineral oil, volatile oil, boronized soap-based dry film, soap-based compounds, etc. With the increasing requirements for high-carbon steel stretching, the shortcomings of traditional lubricants are gradually exposed. For example, mineral oil is difficult to mix, contains harmful and flammable components, and is difficult to clean and directly weld; volatile oil is flammable, toxic, has little protective effect on tools, and increases the VOC content in the workshop; boronized soap-based dry film will produce deposits on the mold, produce borax particles at the stamping site, and become soft and sticky in a humid environment; and soap-based compounds have the disadvantages of easy adhesion at the stamping site, corrosion to soft metals, and foaming during cleaning. This type of stretching oil is not degradable, which limits the use of stretching oil. Therefore, it is urgent to invent a degradable high-carbon steel stretching fluid to meet the higher demands in the field of metal forming and processing technology. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a degradable high-carbon steel drawing fluid.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A degradable high carbon steel drawing liquid comprises the following raw materials in mass fraction: 38-68% modified oleic acid ester, 1-3% rust inhibitor, 3-10% extreme pressure anti-wear agent, 0.1-1% anti-hard water agent, 10-20% surfactant, and the balance is water.

[0008] Furthermore, the anti-hard water agent is one of tetrasodium ethylenediaminetetraacetate (EDTA-4Na) and ether carboxylic acid.

[0009] Furthermore, the surfactant is a mixture of a W / O type surfactant and an O / W type surfactant.

[0010] A degradable high carbon steel drawing fluid is prepared by the following steps:

[0011] A1. Add the modified oleic acid ester into a stirred reactor and heat to 60°C;

[0012] A2. Add W / O type surfactant into the reaction stirring kettle and stir thoroughly;

[0013] A3. Dissolve the O / W surfactant in water and slowly add it dropwise into the reaction kettle, stirring continuously until the solution is clear, uniform and transparent;

[0014] A4. Add rust inhibitor, extreme pressure anti-wear agent and anti-hard water agent to the reactor in sequence. After sufficient stirring, the solution becomes turbid.

[0015] A5. Add an O / W surfactant to the reactor in step A4, stir until the solution is clear, uniform and transparent, and cool to room temperature after it is completely dissolved to obtain a degradable high-carbon steel drawing liquid.

[0016] Furthermore, the rust inhibitor is prepared by the following steps:

[0017] Add organic acid to the reactor, stir thoroughly, then add alcoholamines, introduce N2 protection and heat to 85°C to react for 1 hour. After the reaction is complete, cool to room temperature, cool and crystallize to obtain a rust inhibitor.

[0018] Furthermore, the organic acid is one or both of isooctanoic acid and heneicosenedicarboxylic acid.

[0019] Furthermore, the alcoholamine substance is one of monoethanolamine, triethanolamine, monoisopropanolamine and triisopropanolamine.

[0020] Furthermore, the raw materials are calculated according to mass fraction as follows: 20-30% organic acid, 70-80% alcoholamine substances.

[0021] Furthermore, the extreme pressure anti-wear agent is prepared by the following steps:

[0022] B1. Add petroleum ether and isodecyl alcohol to a three-necked flask, place it in an ice bath, add phosphorus pentoxide in batches while stirring, control the reaction temperature at 55°C, remove the ice bath after the addition is complete, change to a water bath, control the reaction temperature at 50°C, the reaction time is 6h, the reaction is completed, filter and distill under reduced pressure to remove the solvent to obtain diisodecyl pyrophosphate; the ratio of petroleum ether, isodecyl alcohol, and phosphorus pentoxide is 200mL:31.6g:14.1g;

[0023] Isodecyl alcohol and phosphorus pentoxide react, and by controlling the molar ratio of the two to 2:1, diisodecyl pyrophosphate is obtained; the specific reaction process is as follows:

[0024]

[0025] B2. Add diisodecyl pyrophosphate to petroleum ether, stir and mix evenly, then add 2-aminothiazole, react at room temperature for 8 hours, and after the reaction is completed, remove the solvent by distillation under reduced pressure to obtain an extreme pressure antiwear agent; the ratio of petroleum ether, diisodecyl pyrophosphate, and 2-aminothiazole is 200mL:45.8g:20.4g;

[0026] The reaction is exothermic, and no heating is required. Diisodecyl pyrophosphate and 2-aminothiazole react, and by controlling the molar ratio of the two to 2:1, an extreme pressure anti-wear agent is obtained. The specific reaction process is as follows:

[0027]

[0028] The prepared extreme pressure anti-wear agent contains three elements, phosphorus, sulfur and nitrogen, which can work synergistically to greatly enhance its extreme pressure anti-wear performance; in addition, the prepared extreme pressure anti-wear agent is ionic and has a strong polarity compared to ordinary extreme pressure anti-wear agents, which enables it to be effectively adsorbed on the surface of the friction pair and form a friction film during the friction process, thereby reducing friction and wear, further improving anti-wear performance, and improving the picking and cracking of workpieces treated with drawing fluid.

[0029] Further, the modified oleic acid ester is prepared by the following steps:

[0030] S1. Add oleic acid and hydrogen peroxide into a reaction kettle, stir and mix, introduce nitrogen, carry out epoxidation reaction at 60°C for 4 hours, extract and take the upper oil phase, which is intermediate 1;

[0031] S2. Under nitrogen protection, in a reactor, the intermediate 1 obtained in step S1, an organic alcohol and concentrated sulfuric acid (catalyst) are subjected to a ring-opening reaction at 80° C. for 8 hours, the temperature is raised to 120° C., lauric acid is added, and the esterification reaction is carried out for 8 hours to obtain a product;

[0032] S3. After the reaction is completed, the product is subjected to water washing, alkali washing and reduced pressure water removal process to obtain modified oleic acid ester.

[0033] Furthermore, the usage ratio of oleic acid, hydrogen peroxide, organic alcohol, concentrated sulfuric acid and lauric acid is 900g:100g:200g:5g:400g.

[0034] Furthermore, the organic alcohol is one of n-octanol, isooctyl alcohol, n-nonanol and isononanol.

[0035] Beneficial effects of the present invention:

[0036] 1. The rust inhibitor has excellent rust prevention effect on high carbon steel;

[0037] 2. The prepared modified oleic acid ester has higher lubricity than oleic acid itself; and compared with the mineral oil in the traditional stretching fluid, it is degradable;

[0038] 3. The prepared extreme pressure anti-wear agent contains phosphorus, sulfur and nitrogen, which can play a synergistic role, greatly enhance the extreme pressure anti-wear performance of the drawing fluid, and improve the roughening and cracking of the workpiece treated with the drawing fluid;

[0039] Therefore, the stretching liquid prepared by the present invention has good anti-rust effect, high lubricity, degradability and extreme pressure wear resistance, and can improve the phenomenon of hair picking and cracking, and has important application value in the field of metal forming processing technology. DETAILED DESCRIPTION

[0040] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] Example 1

[0042] Preparation of rust inhibitor:

[0043] Add 20% isooctanoic acid into the reactor, stir thoroughly, then add 80% monoethanolamine, introduce N2 protection and heat to 85°C to react for 1 hour. After the reaction is complete, cool to room temperature, cool and crystallize to obtain a rust inhibitor.

[0044] Example 2

[0045] Preparation of rust inhibitor:

[0046] Add 30% of hexone-carbon dibasic acid into the reactor, stir thoroughly, then add 70% of triisopropanolamine, introduce N2 protection and heat to 85°C to react for 1 hour. After the reaction is complete, cool to room temperature, cool and crystallize to obtain a rust inhibitor.

[0047] Example 3

[0048] Preparation of extreme pressure anti-wear agent:

[0049] B1. Add 200 mL of petroleum ether and 31.6 g of isodecyl alcohol to a three-necked flask, place it in an ice bath, add 14.1 g of phosphorus pentoxide in batches while stirring, and control the reaction temperature at 55 ° C. After the addition is completed, remove the ice bath and replace it with a water bath. Control the reaction temperature at 50 ° C. The reaction time is 6 hours. After the reaction is completed, filter and distill under reduced pressure to remove the solvent to obtain diisodecyl pyrophosphate;

[0050] B2. Add 45.8 g of diisodecyl pyrophosphate to 200 mL of petroleum ether, stir and mix well, then add 20.4 g of 2-aminothiazole, react at room temperature for 8 h. After the reaction is complete, remove the solvent by distillation under reduced pressure to obtain an extreme pressure anti-wear agent.

[0051] Example 4

[0052] Preparation of extreme pressure anti-wear agent:

[0053] B1. Add 400 mL of petroleum ether and 63.2 g of isodecyl alcohol to a three-necked flask, place it in an ice bath, add 28.2 g of phosphorus pentoxide in batches while stirring, and control the reaction temperature at 55 ° C. After the addition is completed, remove the ice bath and replace it with a water bath. Control the reaction temperature at 50 ° C. The reaction time is 6 hours. After the reaction is completed, filter and distill under reduced pressure to remove the solvent to obtain diisodecyl pyrophosphate;

[0054] B2. Add 91.6 g of diisodecyl pyrophosphate to 400 mL of petroleum ether, stir and mix well, then add 40.8 g of 2-aminothiazole, react at room temperature for 8 h. After the reaction is complete, remove the solvent by vacuum distillation to obtain an extreme pressure anti-wear agent.

[0055] Example 5

[0056] Preparation of modified oleic acid esters:

[0057] S1, adding 900g of oleic acid and 100g of hydrogen peroxide into a reactor, stirring and mixing, introducing nitrogen, and carrying out epoxidation reaction at 60°C for 4h, extracting and taking the upper oil phase, which is intermediate 1;

[0058] S2. Under nitrogen protection, in a reactor, the intermediate 1 obtained in step S1, 200 g of n-octanol and 5 g of concentrated sulfuric acid were subjected to ring-opening reaction at 80° C. for 8 h, the temperature was raised to 120° C., 400 g of lauric acid was added, and the reaction was esterified for 8 h to obtain the product;

[0059] S3. After the reaction is completed, the product is subjected to water washing, alkali washing and reduced pressure water removal process to obtain modified oleic acid ester.

[0060] Example 6

[0061] Preparation of modified oleic acid esters:

[0062] S1, add 1800g oleic acid and 200g hydrogen peroxide into a reactor, stir and mix, introduce nitrogen, carry out epoxidation reaction at 60°C for 4h, extract and take the upper oil phase, which is intermediate 1;

[0063] S2. Under nitrogen protection, in a reactor, the intermediate 1 obtained in step S1, 400 g of n-nonanol and 10 g of concentrated sulfuric acid were subjected to ring-opening reaction at 80° C. for 8 h, the temperature was raised to 120° C., 800 g of lauric acid was added, and the esterification reaction was carried out for 8 h to obtain the product;

[0064] S3. After the reaction is completed, the product is subjected to water washing, alkali washing and reduced pressure water removal process to obtain modified oleic acid ester.

[0065] Example 7

[0066] A1. Add 68.00% of the modified oleic acid ester prepared in Example 5 into a stirred reaction vessel and heat to 60° C.;

[0067] A2. Add 10.00% sodium petroleum sulfonate into the reaction stirring kettle and stir thoroughly;

[0068] A3. Dissolve 1.50% OP-10 in 10.40% water and slowly add dropwise to the reaction kettle, stirring continuously until the solution is clear, uniform and transparent;

[0069] A4, 1.50% of the rust inhibitor prepared in Example 1, 7.50% of the extreme pressure anti-wear agent prepared in Example 3 and 0.10% of ether carboxylic acid were added to the reaction kettle in sequence, and the solution became turbid after sufficient stirring;

[0070] A5. Add 1.00% OP-10 to the reactor in step A4, stir until the solution is clear, uniform and transparent, then add 50 ppm polyether defoamer, cool to room temperature after complete dissolution, and obtain a degradable high carbon steel drawing liquid.

[0071] The recipe table is as follows:

[0072] raw material Example 7 Rust inhibitor 1.50% Modified oleate 68.00% Oleic acid / Extreme pressure anti-wear agent 7.50% Ether carboxylic acid 0.10% Sodium petroleum sulfonate 10.00% OP-10 2.50% Deionized water 10.40% Polyether defoamer 50ppm

[0073] Example 8

[0074] A1. Add 48.00% of the modified oleic acid ester prepared in Example 6 into a stirred reaction vessel and heat to 60° C.;

[0075] A2. Add 10.00% sodium petroleum sulfonate into the reaction stirring kettle and stir thoroughly;

[0076] A3. Dissolve 3.50% OP-10 in 30.40% water and slowly add dropwise to the reaction kettle, stirring continuously until the solution is clear, uniform and transparent;

[0077] A4, 1.50% of the rust inhibitor prepared in Example 2, 4.5% of the extreme pressure antiwear agent prepared in Example 4 and 0.10% of ether carboxylic acid were added to the reaction kettle in sequence, and the solution became turbid after sufficient stirring;

[0078] A5. Add 2.00% OP-10 to the reactor in step A4, stir until the solution is clear, uniform and transparent, then add 50 ppm polyether defoamer, cool to room temperature after complete dissolution, and obtain a degradable high carbon steel drawing liquid.

[0079] The recipe table is as follows:

[0080] raw material Example 8 Rust inhibitor 1.50% Modified oleate 48.00% Oleic acid / Extreme pressure anti-wear agent 4.5% Ether carboxylic acid 0.10% Sodium petroleum sulfonate 10.00% OP-10 5.50% Deionized water 30.40% Polyether defoamer 50ppm

[0081] Example 9

[0082] A1, adding 38.00% of the modified oleic acid ester prepared in Example 6 into a stirred reaction vessel and heating to 60°C;

[0083] A2. Add 8.00% sodium petroleum sulfonate into the reaction stirring kettle and stir thoroughly;

[0084] A3. Dissolve 4.50% OP-10 in 35.40% water and slowly add dropwise to the reaction kettle, stirring continuously until the solution is clear, uniform and transparent;

[0085] A4, 2.50% of the rust inhibitor prepared in Example 2, 4.5% of the extreme pressure antiwear agent prepared in Example 4 and 0.10% of ether carboxylic acid were added to the reaction kettle in sequence, and the solution became turbid after sufficient stirring;

[0086] A5. Add 7.00% of Siben-80 to the reactor in step A4, stir until the solution is clear, uniform and transparent, then add 50 ppm of polyether defoamer, cool to room temperature after it is completely dissolved, and obtain a degradable high-carbon steel drawing liquid.

[0087] The recipe table is as follows:

[0088] raw material Example 9 Rust inhibitor 2.50% Modified oleate 38.00% Oleic acid / Extreme pressure anti-wear agent 4.50% Ether carboxylic acid 0.10% Sodium petroleum sulfonate 8.00% OP-10 4.50% Siben-80 7.00% Deionized water 35.40% Polyether defoamer 50ppm

[0089] Comparative Example 1

[0090] A commercially available rust inhibitor was used to replace the rust inhibitor in Example 9, and the remaining steps were the same as those in Example 9 to prepare a stretching liquid.

[0091] Comparative Example 2

[0092] Trimethylolpropane oleate was used to replace the modified oleate in Example 9, and the remaining steps were the same as in Example 9.

[0093] Comparative Example 3

[0094] The extreme pressure anti-wear agent in Example 9 was replaced by a commercially available extreme pressure anti-wear agent, and the remaining steps were the same as those in Example 9.

[0095] The performance tests of Examples 7-9, Comparative Examples 1-3 and conventional stretching fluids were performed, and the results are shown in the following table:

[0096]

[0097]

[0098] It can be seen from the above table that the stretching liquid prepared in the embodiment of the present invention has good anti-rust effect, and its lubricity and wear resistance are higher than those of the control example. It is degradable and has good stability, and has important application value in the field of metal forming processing technology.

[0099] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0100] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A degradable high carbon steel drawing fluid, characterized in that: The raw materials include the following mass fractions: 38-68% modified oleic acid ester, 1-3% rust inhibitor, 3-10% extreme pressure anti-wear agent, 0.1-1% anti-hard water agent, 10-20% surfactant, and the balance is water; Wherein, the modified oleic acid ester is prepared by the following steps: S1. Add oleic acid and hydrogen peroxide into a reaction kettle, stir and mix, introduce nitrogen, carry out epoxidation reaction at 60°C for 4 hours, extract and take the upper oil phase, which is intermediate 1; S2. Under nitrogen protection, in a reactor, the intermediate 1 prepared in step S1, an organic alcohol and concentrated sulfuric acid were subjected to a ring-opening reaction at 80° C. for 8 h, the temperature was raised to 120° C., lauric acid was added, and the esterification reaction was carried out for 8 h to obtain a product; S3. After the reaction is completed, the product is subjected to water washing, alkali washing and reduced pressure water removal process to obtain modified oleic acid ester.

2. The degradable high carbon steel drawing liquid according to claim 1, characterized in that: The usage ratio of oleic acid, hydrogen peroxide, organic alcohol, concentrated sulfuric acid and lauric acid is 900g:100g:200g:5g:400g.

3. The degradable high carbon steel drawing liquid according to claim 1, characterized in that: The organic alcohol is one of n-octanol, isooctyl alcohol, n-nonanol and isononanol.

4. The degradable high carbon steel drawing liquid according to claim 1, characterized in that: The extreme pressure anti-wear agent is prepared by the following steps: B1. Add petroleum ether and isodecyl alcohol to a three-necked flask, place it in an ice bath, add phosphorus pentoxide while stirring, control the reaction temperature at 55°C, and after the addition is completed, react at 50°C for 6h. After the reaction is completed, filter and distill under reduced pressure to obtain diisodecyl pyrophosphate; B2. Add diisodecyl pyrophosphate to petroleum ether, stir and mix evenly, then add 2-aminothiazole, react at room temperature for 8 hours, and after the reaction is completed, perform vacuum distillation to obtain an extreme pressure anti-wear agent.

5. The degradable high carbon steel drawing liquid according to claim 4, characterized in that: In step B1, the ratio of petroleum ether, isodecyl alcohol and phosphorus pentoxide is 200 mL: 31.6 g: 14.1 g.

6. The degradable high carbon steel drawing liquid according to claim 4, characterized in that: In step B2, the ratio of petroleum ether, diisodecyl pyrophosphate, and 2-aminothiazole is 200 mL: 45.8 g: 20.4 g.

7. The degradable high carbon steel drawing fluid according to claim 1, characterized in that: The rust inhibitor is prepared by the following steps: Add organic acid to the reactor, stir thoroughly, then add alcoholamines, introduce N2 protection and heat to 85°C to react for 1 hour. After the reaction is complete, cool to room temperature, cool and crystallize to obtain a rust inhibitor.

8. The degradable high carbon steel drawing liquid according to claim 7, characterized in that: The organic acid is one or both of isooctanoic acid and heneicosenedioic acid.

9. The degradable high carbon steel drawing liquid according to claim 7, characterized in that: The alcoholamine substance is one of monoethanolamine, triethanolamine, monoisopropanolamine and triisopropanolamine.

10. The degradable high carbon steel drawing liquid according to claim 7, characterized in that: The raw materials are calculated according to mass fraction as follows: 20-30% organic acid, 70-80% alcohol amine substances.