Organic leather tanning agent with covalent tanning characteristic as well as preparation method and application of organic leather tanning agent

By introducing covalent tanning characteristics into organic leather tanning agents, the multi-point covalent combination of active halogen atoms and collagen is used to solve the problem of insufficient performance of existing chromium-free tanning agents, and higher tanning effects and environmental protection performance are achieved .

CN118996022APending Publication Date: 2024-11-22SICHUAN DECISION CHEM CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411318133.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing chrome-free leather tanning agents have insufficient performance during the tanning process, especially the low binding fastness with leather collagen, which leads to low shrinkage temperature, poor softness and plumpness of the leather, and has not obtained environmental protection problems. Effective solution.

Method used

Using an organic leather tanning agent with covalent tanning characteristics, its molecular structure includes A, B and C structural units. The intermediate is formed by co-condensation reaction of p-aminobenzenesulfonic acid raw materials, phenol raw materials, amino raw materials and formaldehyde. , and graft reaction with tripolymer halide cyanide to improve the reactivity of active halogen atoms and achieve multi-point covalent binding with keratin collagen.

Benefits of technology

Improves the fastness of the bonding of organic leather tanning agent and leather collagen, enhances the shrinkage temperature, softness and plumpness of the leather, can be used as a separate tanning agent, is more environmentally friendly than chrome tanning agent, and is in the manufacture of high-performance leather There are significant advantages when it is.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996022A_ABST
    Figure CN118996022A_ABST
Patent Text Reader

Abstract

The invention discloses an organic leather tanning agent with covalent tanning characteristics and a preparation method and application thereof, and relates to the technical field of leather tanning agents. The matrix of the C structural unit contains active amino groups, and the reaction activity of the active amino groups and active halogen atoms is higher, so that the grafting capacity is higher, the active halogen atoms can be prevented from being hydrolyzed, and the active halogen atoms can be quantitatively grafted on the active amino groups of the C structural unit. According to the organic leather tanning agent, the active halogen atoms on the C structural units can be combined with the leather collagen of the raw leather in a covalent bond mode, and the multiple C structural units in the organic leather tanning agent and the leather collagen of the raw leather form multi-point covalent binding, so that the binding strength of the organic leather tanning agent and the leather collagen is improved; other groups in the organic leather tanning agent can form hydrogen bonds, ionic bonds and the like with leather, so that the binding strength of the organic leather tanning agent and the leather is further improved, and the shrinkage temperature, softness and fullness of finished leather are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of leather tanning agents, and in particular to an organic leather tanning agent with covalent tanning properties, a preparation method and application thereof. Background Art

[0002] Chemicals that cause raw hides to tan are collectively referred to as leather tanning agents. The principle of tanning is to physically and chemically combine leather tanning agents with various functional groups in the collagen of the hides, causing the raw hides to denature into leather. The occurrence of tanning is mainly reflected in the increase of the shrinkage temperature of the bare hides, the enhancement of the physical and mechanical strength of the leather and its resistance to heat, microorganisms, and chemical agents, and the leather has good sensory properties and usability.

[0003] Existing leather tanning agents are mainly divided into two categories: inorganic and organic. Inorganic tanning agents are inorganic salts represented by chromium salts, which are the most widely used tanning agents at present. They have the advantages of high shrinkage temperature and good comprehensive performance. However, the tanning process will produce chromium-containing wastewater, waste residue and sludge, which is not conducive to environmental protection. Therefore, the development and promotion of good performance chrome-free tanning agents and tanning methods is the only way to solve the serious defects of the current chrome tanning technology. It is also a technical problem that needs to be solved urgently in the leather industry and one of the very important research hot topics.

[0004] Existing organic leather tanning agents mainly include vegetable tanning agents and synthetic tanning agents. Vegetable tanning agents are also called tannin extracts. The finished leather tanned with them is stiff and has very limited uses. Synthetic tanning agents are tanning agents prepared by organic chemical methods. Due to their low bonding strength with leather collagen, the shrinkage temperature of the finished leather is relatively low, and the comprehensive properties such as softness and fullness are not as good as chrome-tanned leather. Currently, they are rarely used alone as main tanning agents for tanning, and are generally used as retanning agents to improve the performance of chrome-tanned leather.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The purpose of the present invention is to provide an organic leather tanning agent with covalent tanning properties and a preparation method and application thereof.

[0007] The present invention is achieved in that:

[0008] In a first aspect, the present invention provides an organic leather tanning agent having covalent tanning properties, wherein the molecular structure of the organic leather tanning agent comprises an A structural unit, a B structural unit and a C structural unit.

[0009] The structure of the A structural unit is:

[0010] The structure of the B structural unit is

[0011] The structure of the C structural unit is

[0012] Among them, R1 includes H, -SO3H, -CH2-SO3H, C 1~4 Alkyl, -COOH and Any of .

[0013] R2 includes H, —OH, and C 1~4 Any of the alkyl groups.

[0014] R3 includes Any of .

[0015] R4 includes Any of .

[0016] a is an integer greater than or equal to 0, b is 0 or 1, and a and b cannot be 0 at the same time; c and n are both integers greater than or equal to 1, X is F or Cl, and M is any one of H, alkali metal cation, tertiary amine cation or quaternary ammonium cation.

[0017] In a second aspect, the present invention provides a method for preparing an organic leather tanning agent as described in any of the aforementioned embodiments, comprising subjecting an aminobenzenesulfonic acid raw material, a phenol raw material, an amino raw material and formaldehyde to a co-condensation reaction to obtain an intermediate, wherein the molecular structure of the intermediate includes a polymerization unit shown in structure II, and then grafting the intermediate with tricyanamide.

[0018] Structure II is:

[0019] In a third aspect, the present invention provides an organic leather tanning agent according to any one of the aforementioned embodiments or an organic leather tanning agent prepared by the preparation method according to any one of the aforementioned embodiments in the field of rawhide tanning.

[0020] The present invention has the following beneficial effects:

[0021] The present invention provides an organic leather tanning agent with covalent tanning properties, and a preparation method and application thereof. An active halogen structure is grafted into a C structural unit of the organic leather tanning agent. The matrix of the C structural unit contains an active amino group, and the active amino group has a higher reactivity with the active halogen atom, so the grafting ability is stronger, and the hydrolysis of the active halogen atom can be avoided, so that the active halogen atom can be quantitatively grafted onto the active amino group of the C structural unit. The active halogen atom on the C structural unit can be combined with the skin collagen of the raw hide in a covalent bond manner, and multiple C structural units in the organic leather tanning agent form multi-point covalent bonds with the skin collagen of the raw hide, thereby improving the bonding strength of the organic leather tanning agent with the skin collagen. In addition, the sulfonic acid group on the C structural unit can also form an ionic bond with the skin fiber, further improving the bonding strength of the organic leather tanning agent with the leather, and improving the shrinkage temperature, softness and fullness of the finished leather. It can be used as a separate tanning agent and is more environmentally friendly than a chrome tanning agent. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0023] Figure 1 Infrared spectra of the unmodified tanning agents provided in Examples 1, 2, 5, and 6 of the present invention;

[0024] Figure 2 Infrared spectra of the modified organic leather tanning agents provided in Examples 1, 2, 5, and 6 of the present invention. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0026] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0027] In a first aspect, the present invention provides an organic leather tanning agent having covalent tanning properties, wherein the molecular structure of the organic leather tanning agent comprises an A structural unit, a B structural unit and a C structural unit;

[0028] The structure of the A structural unit is:

[0029] The structure of the B structural unit is

[0030] The structure of the C structural unit is

[0031] The A structural unit, the B structural unit and the C structural unit are interconnected and combined to form the polymer molecular structure of the organic leather tanning agent.

[0032] Among them, R1 includes H, -SO3H, -CH2-SO3H, C 1~4 Alkyl, -COOH and Any of .

[0033] R2 includes H, —OH, and C 1~4 Any of the alkyl groups.

[0034] R3 includes

[0035] R4 includes Any of .

[0036] —*: represents a polymer repeating unit segment; a is an integer greater than or equal to 0, b is 0 or 1, and a and b cannot be 0 at the same time; c and n are both integers greater than or equal to 1, X is F or Cl, and M is any one of H, alkali metal cation, tertiary amine cation or quaternary ammonium cation.

[0037] By grafting an active halogen structure into the C structural unit of the organic leather tanning agent, the matrix of the C structural unit contains an active amino group, and the active amino group has a higher reactivity with the active halogen atom, so the grafting ability is stronger, and the hydrolysis of the active halogen atom can be avoided, so that the active halogen atom can be quantitatively grafted onto the active amino group of the C structural unit. The active halogen atom on the C structural unit can be combined with the skin collagen of the raw hide in the form of a covalent bond, and multiple C structural units in the organic leather tanning agent form multi-point covalent bonds with the skin collagen of the raw hide, thereby improving the bonding strength between the organic leather tanning agent and the skin collagen. In addition, the sulfonic acid group on the C structural unit can also form an ionic bond with the skin fiber, further improving the bonding strength between the organic leather tanning agent and the leather, and improving the shrinkage temperature, softness and fullness of the finished leather. It can be used as a separate tanning agent and is more environmentally friendly than chrome tanning agents.

[0038] In an optional embodiment, the connection mode between the A structural unit, the B structural unit and the C structural unit in the organic leather tanning agent can be to connect the A structural unit, the B structural unit and the C structural unit in sequence, or to connect the A structural unit, the C structural unit and the B structural unit in sequence, etc.

[0039] In an optional embodiment, in order to further ensure the tanning effect, the general structural formula of the organic leather tanning agent is as shown in the following structure:

[0040] structure:

[0041] In the existing organic leather tanning agents that use active halogen atoms as the key groups for leather tanning, the technology usually involves reacting raw materials containing active halogen atoms, such as cyanuric halide, with the phenolic hydroxyl group in the A structural unit to improve the covalent tanning performance of the general phenolic synthetic tanning agent. However, during the reaction process, due to the low reactivity of the phenolic hydroxyl group, the cyanuric halide will be partially hydrolyzed during the grafting reaction in an aqueous medium, and it is impossible to completely graft all of the cyanuric halide to the phenolic hydroxyl group of the A structural unit, resulting in the actual reaction process not being a quantitative reaction. Part of the cyanuric halide that should be grafted on the phenolic hydroxyl group will be directly hydrolyzed, causing the actual tanning effect of the organic leather tanning agent to be different from the theoretical tanning effect, resulting in poor actual tanning effect, etc.

[0042] The organic leather tanning agent provided by the present invention has a structure as shown in the structure. It is specially designed to embed the highly reactive p-aminobenzenesulfonic acid structural unit (i.e., C structural unit) into the molecular structure of the synthetic tanning agent, and then the reactive amino group of the C structural unit is reacted with cyanuric halide, and its reactive activity exceeds the reactive activity with the phenolic hydroxyl group. Therefore, it can not only improve the reaction efficiency, but also avoid the hydrolysis of cyanuric halide to the greatest extent, so that the cyanuric halide can react quantitatively, the actual tanning effect is better, and the finished leather with better performance can be obtained.

[0043] Preferably, R1 includes H, -SO3H, -CH2-SO3H, -COOH and Any of .

[0044] R2 includes H or -OH.

[0045] R3 is

[0046] a is an integer greater than or equal to 0, b is 0 or 1, and a and b cannot be 0 at the same time; c is an integer greater than or equal to 1, X is F or Cl, and M is H or an alkali metal cation.

[0047] In a second aspect, the present invention provides a method for preparing an organic leather tanning agent according to any one of the aforementioned embodiments, comprising subjecting a p-aminobenzenesulfonic acid raw material, a phenol raw material, an amino raw material and formaldehyde to a co-condensation reaction to obtain an intermediate, wherein the molecular structure of the intermediate includes a polymerization unit shown in structure II, and then subjecting the intermediate to a grafting reaction with tricyanamide;

[0048] Structure II is:

[0049] The values ​​of a, b, c and n can be adjusted according to the amount of raw materials added to the reaction, as long as they are within the aforementioned required range.

[0050] In an optional embodiment, the co-condensation reaction includes: adding phenol raw materials and / or amino raw materials to a system of p-aminobenzenesulfonic acid raw materials and a pH regulator, then mixing at a first reaction temperature to obtain a first solution, adding formaldehyde to the first solution, and then heating to carry out a co-condensation reaction.

[0051] Among them, the role of phenol raw materials is mainly to form basic molecular units of general phenolic synthetic tanning agents, such as A structural unit, which embodies the tanning property of hydrogen bonds of phenolic hydroxyl groups similar to general phenolic synthetic tanning agents, and undergoes condensation reaction with p-aminobenzenesulfonic acid raw materials through formaldehyde to obtain modified synthetic tanning agents containing active amino structural units (C structural units). The p-aminobenzenesulfonic acid raw materials also impart good water solubility to the condensation polymer. The role of amino raw materials is mainly to undergo co-condensation reaction with phenol raw materials or p-aminobenzenesulfonic acid raw materials to introduce new functional groups into the molecular structure. According to the specific properties of the raw materials and the structural design requirements, either phenol raw materials or amino raw materials can be selected, and preferably both are selected.

[0052] In the preparation method of the organic leather tanning agent provided by the present invention, the intermediate prepared has active phenolic hydroxyl groups, aromatic sulfonic acid and other active groups of a general aromatic synthetic tanning agent, and these active groups can produce certain hydrogen bonds and ionic bonds with leather, have tanning properties and tanning effects in the traditional sense, and are a small molecule polymer with potential reactivity. In addition, the aminoaromatic sulfonic acid structure in the C structural unit can not only give the synthetic tanning agent water solubility, but also serve as a grafting reaction site for modification of active halogen atoms, introduce active halogen atoms that can produce covalent bonds with leather into the aminoaromatic sulfonic acid structure, and introduce active halogen atoms into the intermediate by reacting the intermediate with cyanuric halide. Since the active halogen atoms are more likely to react with the active amino groups in the active C structural unit, they can be quickly and completely quantitatively grafted into the C structural unit, so that the tanning mechanism and tanning effect of the organic leather tanning agent obtained by the organic leather tanning agent undergo qualitative changes, and the organic leather tanning agent can be used not only as a single tanning agent, but also for leather retanning and filling, and has great potential in leather tanning processing.

[0053] Preferably, water is added to the co-polycondensation reaction, and more preferably, the water is deionized water. Since the pH regulator contains some water, it can be used as a solvent. In order to ensure that the raw materials in the first solution can be fully dissolved, some water can also be added as a solvent.

[0054] Preferably, the p-aminobenzenesulfonic acid raw materials include aromatic aminosulfonic acid compounds or their salts and aromatic aminocarboxylic acid compounds or their salts, and the salts are sodium salts or potassium salts.

[0055] Preferably, the aromatic aminosulfonic acid compound includes any one of p-aminobenzenesulfonic acid, 2,4-diaminobenzenesulfonic acid and p-aminobenzoic acid.

[0056] Preferably, the aromatic aminocarboxylic acid compound includes any one of aminobenzoic acid, aminophenylacetic acid or aminophenylpropionic acid.

[0057] Preferably, the phenolic raw material includes at least one of phenol, cresol, ethylphenol, xylenol and its sulfonate, 4,4-dihydroxydiphenyl sulfone, salicylic acid, p-hydroxybenzoic acid, and sulfosalicylic acid.

[0058] Preferably, the amino raw material includes at least one of urea, carbamate, glycine, lysine and aminoethanesulfonic acid.

[0059] Preferably, the concentration of formaldehyde is 35-40%.

[0060] Preferably, in order to facilitate the dissolution of each raw material, the first reaction temperature is 60-70°C.

[0061] Preferably, during the process of adding formaldehyde, the temperature of the system is maintained at the first reaction temperature, which can improve the safety of the reaction system. Some raw material combinations will have a more obvious release of reaction heat.

[0062] Preferably, after adding formaldehyde, the temperature is raised to 90-95° C. to further complete the co-condensation reaction, and the reaction time is 3-5 hours.

[0063] Preferably, the co-condensation reaction conditions include either acidic conditions or alkaline conditions, and the reaction conditions can be achieved by selecting a pH adjuster. For example, for a co-condensation reaction under acidic conditions, an acid is selected as a pH adjuster, and for a co-condensation reaction under alkaline conditions, a base is selected as a pH adjuster.

[0064] The specific selection of co-condensation conditions is related to the type of raw materials. When the raw materials can only undergo co-condensation reaction under acidic conditions, the pH adjuster is an acid. When the raw materials can only undergo co-condensation reaction under alkaline conditions, the pH adjuster is a base.

[0065] In an optional embodiment, when the pH adjuster is an acid, the pH of the first solution is ≤3, preferably, pH ≤2.

[0066] Moreover, the weight ratio of the aminobenzenesulfonic acid raw material, the phenol raw material, the amino raw material, water and the pH adjuster is 80-120:30-300:0-62:90-400:5-20.

[0067] Preferably, the p-aminobenzenesulfonic acid raw material is any one of p-aminobenzenesulfonic acid, 2,4-diaminobenzenesulfonic acid and p-aminobenzoic acid, and the p-aminobenzenesulfonic acid raw materials are more suitable for co-condensation under acidic conditions.

[0068] Preferably, the acid is any one of 50% sulfuric acid, 36.5% concentrated hydrochloric acid or formic acid;

[0069] Preferably, the weight ratio of formaldehyde to p-aminobenzenesulfonic acid raw materials is 60-120:80-120.

[0070] In an alternative embodiment, when the pH adjuster is a base, the pH of the first solution is 9-11.

[0071] The weight ratio of the aminobenzenesulfonic acid raw material, the phenol raw material, the amino raw material, water and the pH regulator is 80-120:0-300:0-105:0-400:5-200.

[0072] Preferably, the p-aminobenzenesulfonic acid raw material can be any one of sodium p-aminobenzenesulfonate, potassium p-aminobenzenesulfonate, sodium 2,4-diaminobenzenesulfonate, sodium p-aminobenzoate and potassium p-aminobenzoate. The above p-aminobenzenesulfonic acid raw materials are more suitable for co-condensation under alkaline conditions.

[0073] Preferably, the base is any one of NaOH, Na2CO3 or KOH.

[0074] Preferably, the weight ratio of formaldehyde to p-aminobenzenesulfonic acid raw materials is 60-240:80-120.

[0075] In an optional embodiment, after the co-polycondensation reaction is completed, the system temperature is lowered to 48-52° C., the pH of the system is adjusted to 6-8, and sodium metabisulfite is added to the system and stirred for 20-40 minutes;

[0076] Preferably, the weight ratio of sodium pyrosulfite to p-aminobenzenesulfonic acid raw materials is 2-30:80-120.

[0077] Furthermore, since formaldehyde is used as one of the raw materials for the reaction during the co-condensation reaction, when formaldehyde remains in the organic leather tanning agent, the formaldehyde enters the leather during the tanning process, which will cause the formaldehyde content of the leather to exceed the standard. In order to avoid this situation, sodium metabisulfite is added to the reaction system after the co-condensation reaction is completed to remove residual formaldehyde and improve the safety of leather use.

[0078] In an optional embodiment, the process of grafting active halogen atoms comprises reacting the intermediate with excess cyanuric halide at 0-5° C., maintaining the pH of the reaction system at 6-8 during the reaction, and adjusting the pH of the system to 4-6 after the reaction.

[0079] Preferably, the pH of the reaction system is controlled by adding acid and / or base. For example, when the pH is lower than the required range, an alkaline substance such as NaOH is added to the system to increase the pH. When the pH is higher than the required range, an acidic substance such as sulfuric acid is added to the system to lower the pH.

[0080] Preferably, during the active halogen atom grafting reaction process, maintaining the pH of the reaction system at 6 to 8 is conducive to the smooth grafting of cyanuric halide to the active amino site and the smooth progress of the grafting reaction.

[0081] In order to ensure that the pH of the reaction system is 6-8, soda ash is added during the reaction to control the pH of the system and promote the reaction of cyanuric halide with active amino sites.

[0082] Since the three halogen atoms of cyanuric halide have different reaction temperatures, the reaction temperature of the first halogen atom is generally 0-5°C, so controlling the reaction temperature at 0-5°C is conducive to the smooth grafting of cyanuric halide. The reaction temperatures of the remaining two halogen atoms in cyanuric halide are around 40°C and 80°C, respectively. Therefore, the tanning temperature is generally around 40°C, so that the active halogen atoms in the organic leather tanning agent can react with the skin collagen and combine in the form of covalent bonds, thereby improving the tanning effect of the organic leather tanning agent.

[0083] Since a large amount of cyanuric halide is added, it can completely react the intermediate to generate more organic leather tanning agents. The remaining cyanuric halide can be filtered out for next use, or a small amount of p-aminobenzenesulfonic acid raw materials, such as sodium p-aminobenzenesulfonate monomer, can be added to the system to react the remaining cyanuric halide. Excessive cyanuric halide is beneficial to ensure that the active amino site reacts completely and ensures the stable storage of the product, avoiding the reaction of the remaining active amino group with the second chlorine atom during storage of the product, resulting in unstable product or loss of tanning properties.

[0084] Preferably, the molar ratio of the active amino group in the intermediate to the cyanuric halide is 1:0.8-10, more preferably 1:1-1.05.

[0085] Preferably, the cyanuric halide is cyanuric chloride or cyanuric fluoride, more preferably cyanuric chloride.

[0086] Preferably, after adjusting the pH of the system to 4-6, wait for the system to naturally warm up to room temperature, for example, 20-25° C., and stir for 1 hour to obtain a clear and transparent aqueous solution, which is the organic leather tanning agent provided by the present invention.

[0087] The organic leather tanning agent provided by the present invention has more ways of combining with leather fibers, and the combination is more firm, while maintaining the filling feel and other properties unchanged, and has better heat resistance and light resistance stability, and has a certain tanning effect, and has obvious advantages in manufacturing high-performance leathers such as white leather or light-colored leather. In addition, the organic leather tanning agent provided by the present invention can tan raw hides within the pH range of 5.0 to 9.5 without pre-pickling or de-pickling of pickled hides, and has a wider range of applications, and reduces the processing technology of raw hides and the discharge of wastewater during the pickling process, and the tanning process is more environmentally friendly. Leather, fur or bare skin tanned by the organic leather tanning agent provided by the present invention is convenient for further processing.

[0088] In a third aspect, the present invention provides an organic leather tanning agent according to any one of the aforementioned embodiments or an organic leather tanning agent prepared by the preparation method according to any one of the aforementioned embodiments in the field of rawhide tanning.

[0089] Example 1

[0090] This embodiment provides an organic leather tanning agent with covalent tanning properties, and its structure is: a>1, c>1, and a and c are both integers.

[0091] This embodiment also provides a method for preparing the above-mentioned organic leather tanning agent, comprising the following steps:

[0092] S01. Co-condensation reaction

[0093] The co-condensation reaction is carried out in a constant temperature reactor equipped with a thermometer, a N2 inlet tube, a reflux condenser and a mechanical stirring device.

[0094] Add 30 parts by weight of distilled water, 80 parts by weight of sodium p-aminobenzenesulfonate and 65 parts by weight of phenol into the above-mentioned constant temperature reactor, and then add 5 parts by weight of 30% NaOH solution to adjust the pH of the system to 10-11, heat the system to 60°C and stir to dissolve the raw materials to obtain the first solution. Control the temperature of the first solution not to exceed 70°C, and slowly drop 126 parts by weight of 37% formaldehyde solution during this process. After the dropwise addition is completed, heat the system to 90-95°C for insulation reaction, and the total insulation time is 3 hours. After the insulation is completed, cool the system to 50°C to obtain an intermediate, which is recorded as 1-a.

[0095] S02, Grafting Reaction

[0096] Take 100g of the intermediate obtained in step S01 and pre-freeze it to 0°C. Then add 20 parts by weight of distilled water to a 500ml glass beaker and cool it in an ice water bath at 0-5°C. After cooling, add 22 parts by weight of cyanuric chloride and stir with a disperser to obtain a cyanuric chloride dispersion slurry. Keeping the rapid stirring condition, slowly pour the pre-cooled intermediate 1-a into the cyanuric chloride dispersion slurry, maintain the system temperature at 0-5°C and continue stirring. When the system is acidic when tested with a wide range of test paper, add 6 parts by weight of soda ash in batches to maintain the pH value of the system between 6 and 8 until the grafting modification reaction is completed.

[0097] In this embodiment, the molar ratio of the active amino group in the aminoaromatic sulfonic acid structure to cyanuric chloride is 1:1.05. The conversion rate of cyanuric chloride was measured by sampling and was close to 100%. Unreacted cyanuric chloride can be filtered out and collected by filtration, and circulated into the production of the next batch. For the economical applicability of production, this embodiment adopts the addition of 1.4 parts by weight of sodium p-aminobenzenesulfonate and 0.32 parts by weight of sodium carbonate to react with excess cyanuric chloride at 0-5°C, and continues to stir for 1h until the cyanuric chloride reacts completely. After the reaction is completed, the pH value of the product is adjusted to 4-6, and the temperature is naturally raised to 20°C and continued to stir for 1 hour. The 1% aqueous solution is sampled and tested to be clear and transparent without white insoluble particles. The organic leather tanning agent provided in this embodiment is obtained by filtration, which is recorded as 1#.

[0098] Example 2

[0099] This embodiment provides an organic leather tanning agent with covalent tanning properties, and its structure is: a>1, c>1, and a and c are both integers, and b=1.

[0100] This embodiment also provides a method for preparing the above-mentioned organic leather tanning agent, comprising the following steps:

[0101] S01. Co-condensation reaction

[0102] The co-condensation reaction is carried out in a constant temperature reactor equipped with a thermometer, a N2 inlet tube, a reflux condenser and a mechanical stirring device.

[0103] Add 90 parts by weight of distilled water, 104 parts by weight of p-aminobenzenesulfonic acid, 62 parts by weight of urea and 75 parts by weight of bisphenol S into the above-mentioned constant temperature reactor, then add 15 parts by weight of 50% sulfuric acid solution to adjust the pH of the system to <2, heat the system to 60°C and stir to dissolve the raw materials to obtain the first solution. Control the temperature of the first solution not to exceed 70°C, slowly drop 121 parts by weight of 37% formaldehyde solution in this process, after the dropwise addition is completed, heat the system to 90-95°C for insulation reaction, the total insulation time is 4 hours, sample and test water solubility, the aqueous solution becomes transparent or is neutralized with 10% sodium carbonate solution to pH 6-7 and is completely transparent, and there is no granular insoluble matter, the insulation is completed, the system is cooled to 50°C, and then 78 parts by weight of 30% NaOH solution is added to the system to adjust the pH of the system to 8, and 9 parts by weight of sodium pyrosulfite is added to the system and stirred for 30 minutes to obtain an intermediate, which is recorded as 2-a.

[0104] S02, Grafting Reaction

[0105] Take 100g of the intermediate obtained in step S01 and pre-freeze it to 0°C. Then add 22 parts by weight of distilled water to a 500ml glass beaker and cool it in an ice water bath at 0-5°C. After cooling, add 21 parts by weight of cyanuric chloride and stir with a disperser to obtain a cyanuric chloride dispersion slurry. Maintaining rapid stirring conditions, slowly pour the pre-cooled intermediate 2-a into the cyanuric chloride dispersion slurry, maintain the system temperature at 0-5°C and continue stirring. When the system is acidic when tested with a wide range of test paper, add 5.7 parts by weight of soda ash in batches to maintain the pH value of the system between 6 and 8 until the grafting modification reaction is completed.

[0106] In this embodiment, the molar ratio of the active amino group in the aminoaromatic sulfonic acid structure to cyanuric chloride is 1:1.05. The conversion rate of cyanuric chloride was measured by sampling and was close to 100%. Unreacted cyanuric chloride can be filtered out and collected by filtration, and circulated into the production of the next batch. For the economical applicability of production, this embodiment adopts the addition of 1.26 parts by weight of sodium p-aminobenzenesulfonate and 0.3 parts by weight of sodium carbonate to react with excess cyanuric chloride at 0-5°C, and continues to stir for 1h until the cyanuric chloride reacts completely. After the reaction is completed, the pH value of the product is adjusted to 4-6, and the temperature is naturally raised to 20°C and continued to stir for 1 hour. The 1% aqueous solution sampled and tested is clear and transparent, without white insoluble particles. The organic leather tanning agent provided in this embodiment is obtained by filtration, which is recorded as 2#.

[0107] Example 3

[0108] This embodiment provides a method for preparing an organic leather tanning agent with covalent tanning properties, which comprises the following steps:

[0109] S01. Co-condensation reaction

[0110] The co-condensation reaction is carried out in a constant temperature reactor equipped with a thermometer, a N2 inlet tube, a reflux condenser and a mechanical stirring device.

[0111] Add 80 parts by weight of distilled water, 92 parts by weight of sodium p-aminobenzenesulfonate and 60 parts by weight of phenol into the above-mentioned constant temperature reactor, then add 5 parts by weight of 30% NaOH solution to adjust the pH of the system to 10-11, heat the system to 60°C and stir to dissolve the raw materials to obtain the first solution. Control the temperature of the first solution not to exceed 70°C, slowly drop 60 parts by weight of 37% formaldehyde solution in this process, after the dropwise addition is completed, heat the system to 90-95°C for insulation reaction, and the total insulation time is 3 hours. After the insulation is completed, post-treatment is carried out, the system is cooled to 50°C, and then 78 parts by weight of 30% NaOH solution is added to the system to adjust the pH of the system to 8, 3 parts by weight of sodium pyrosulfite are added to the system, stirred for 30 minutes, unreacted impurities are filtered and discarded, and the remaining material is an intermediate, recorded as 3-a.

[0112] 3-a molar ratio n 苯酚 :n ABSNa =1.55,n 甲醛 / (n 苯酚 +n ABSNa )=0.71, therefore, the content of sodium p-aminobenzenesulfonate (ABSNa) is 37.2%; the molar ratio n in 1-a 苯酚 :n ABSNa =1.92, n 甲醛 / (n 苯酚 +n ABSNa )=1.50, therefore, the content of sodium p-aminobenzenesulfonate (ABSNa) is 26.1%. 3-a and 1-a have the same raw material types, but the ratios between the raw materials are different, so that the molecular structures and molecular weights of 1-a and 3-a are different.

[0113] S02, Grafting Reaction

[0114] Take 100g of the intermediate obtained in step S01 and pre-freeze it to 0°C. Then add 30 parts by weight of distilled water to a 500ml glass beaker and cool it in an ice water bath at 0-5°C. After cooling, add 30 parts by weight of cyanuric chloride and stir with a disperser to obtain a cyanuric chloride dispersion slurry. Keeping the rapid stirring condition, slowly pour the pre-cooled intermediate 3-a into the cyanuric chloride dispersion slurry, maintain the system temperature at 0-5°C and continue stirring. When the system is acidic when tested with a wide range of test paper, add 7 parts by weight of soda ash in batches to maintain the pH value of the system between 6 and 8 until the grafting modification reaction is completed.

[0115] In this embodiment, the molar ratio of the active amino group in the aminoaromatic sulfonic acid structure to cyanuric chloride is 1:1.05. The conversion rate of cyanuric chloride was measured by sampling and was close to 100%. Unreacted cyanuric chloride can be filtered out and collected by filtration, and circulated into the production of the next batch. For the economical applicability of production, this embodiment adopts the addition of 6.9 parts by weight of sodium p-aminobenzenesulfonate and 1.6 parts by weight of sodium carbonate to react with excess cyanuric chloride at 0-5°C, and continues to stir for 1h until the cyanuric chloride reacts completely. After the reaction is completed, the pH value of the product is adjusted to 4-6, and the temperature is naturally raised to 20°C and continued to stir for 1 hour. The 1% aqueous solution sampled and tested is clear and transparent, without white insoluble particles. The organic leather tanning agent provided in this embodiment is obtained by filtration, which is recorded as 3#.

[0116] Example 4

[0117] This embodiment provides a method for preparing an organic leather tanning agent with covalent tanning properties, and the steps are similar to those of embodiment 3, except that:

[0118] S01. The amounts of raw materials added in the co-condensation reaction are: 115 parts by weight of distilled water, 92 parts by weight of sodium p-aminobenzenesulfonate, 99 parts by weight of bisphenol S, and 65 parts by weight of 37% formaldehyde solution. The intermediate obtained by the co-condensation reaction is denoted as 4-a.

[0119] S02, the amount of raw materials added in the grafting reaction is: 22 parts by weight of distilled water, 21 parts by weight of cyanuric chloride, 7 parts by weight of soda ash; 1.62 parts by weight of sodium p-aminobenzenesulfonate and 0.5 parts by weight of sodium carbonate are added again. The organic leather tanning agent obtained after the grafting reaction is recorded as 4#.

[0120] Example 5

[0121] This embodiment provides a method for preparing an organic leather tanning agent with covalent tanning properties, and the steps are similar to those of embodiment 3, except that:

[0122] S01. The amounts of raw materials added in the co-condensation reaction are: 30 parts by weight of distilled water, 80 parts by weight of sodium p-aminobenzenesulfonate, 48 parts by weight of salicylic acid, 50 parts by weight of 30% NaOH, 70 parts by weight of 37% formaldehyde solution and 2 parts by weight of sodium pyrosulfite. The intermediate obtained by the co-condensation reaction is recorded as 5-a.

[0123] S02, the amount of raw materials added in the grafting reaction is: 20 parts by weight of distilled water, 25 parts by weight of cyanuric chloride, 6.6 parts by weight of soda ash; 1.62 parts by weight of sodium p-aminobenzenesulfonate and 0.62 parts by weight of sodium carbonate are added again. The organic leather tanning agent obtained after the grafting reaction is recorded as 5#.

[0124] Example 6

[0125] This embodiment provides a method for preparing an organic leather tanning agent with covalent tanning properties, and the steps are similar to those of embodiment 3, except that:

[0126] S01. The amounts of raw materials added in the co-condensation reaction are: 25 parts by weight of distilled water, 100 parts by weight of sodium p-aminobenzenesulfonate, 29 parts by weight of glycine, 50 parts by weight of 30% NaOH and 62 parts by weight of 37% formaldehyde solution. The intermediate obtained by the co-condensation reaction is denoted as 6-a.

[0127] S02, the amount of raw materials added in the grafting reaction is: 32 parts by weight of distilled water, 32 parts by weight of cyanuric chloride, 8.5 parts by weight of soda ash; 2.9 parts by weight of sodium p-aminobenzenesulfonate and 0.7 parts by weight of sodium carbonate are added again. The organic leather tanning agent obtained after the grafting reaction is recorded as 6#.

[0128] Example 7

[0129] This embodiment provides a method for preparing an organic leather tanning agent with covalent tanning properties, and the steps are similar to those of embodiment 3, except that:

[0130] S01. The amounts of raw materials added in the co-polycondensation reaction are: 32 parts by weight of distilled water, 100 parts by weight of sodium p-aminobenzenesulfonate, 40 parts by weight of phenol, 50 parts by weight of glycine, 86 parts by weight of 30% NaOH, 108 parts by weight of 37% formaldehyde solution and 5 parts by weight of sodium pyrosulfite. The intermediate obtained by the co-polycondensation reaction is recorded as 7-a.

[0131] S02, the amount of raw materials added in the grafting reaction is: 22 parts by weight of distilled water, 21 parts by weight of cyanuric chloride, 5.6 parts by weight of soda ash; 1.84 parts by weight of sodium p-aminobenzenesulfonate and 0.42 parts by weight of sodium carbonate are added again. The organic leather tanning agent obtained after the grafting reaction is recorded as 7#.

[0132] Example 8

[0133] This embodiment provides a method for preparing an organic leather tanning agent with covalent tanning properties, and the steps are similar to those of embodiment 3, except that:

[0134] S01, the amounts of raw materials added in the co-condensation reaction are: 100 parts by weight of sodium p-aminobenzenesulfonate, 30 parts by weight of phenol, 48 parts by weight of glycine, 25 parts by weight of bisphenol S, 83 parts by weight of 30% NaOH, 104 parts by weight of 37% formaldehyde solution and 5 parts by weight of sodium pyrosulfite. The intermediate obtained by the co-condensation reaction is recorded as 8-a.

[0135] S02, the amount of raw materials added in the grafting reaction is: 22 parts by weight of distilled water, 22 parts by weight of cyanuric chloride, 5.9 parts by weight of soda ash; 1.7 parts by weight of sodium p-aminobenzenesulfonate and 0.4 parts by weight of sodium carbonate are added again. The organic leather tanning agent obtained after the grafting reaction is recorded as 8#.

[0136] Example 9

[0137] This embodiment provides a method for preparing an organic leather tanning agent with covalent tanning properties, and the steps are similar to those of embodiment 3, except that:

[0138] S01, the amounts of raw materials added in the co-condensation reaction are: 100 parts by weight of sodium p-aminobenzenesulfonate, 30 parts by weight of phenol, 58 parts by weight of glycine, 25 parts by weight of bisphenol S, 20 parts by weight of salicylic acid, 122 parts by weight of 30% NaOH, 104 parts by weight of 37% formaldehyde solution and 5 parts by weight of sodium pyrosulfite. The intermediate obtained by the co-condensation reaction is recorded as 9-a.

[0139] S02, the amounts of raw materials added in the grafting reaction are: 10 parts by weight of distilled water, 18 parts by weight of cyanuric chloride, 4.9 parts by weight of soda ash; 1.0 parts by weight of sodium p-aminobenzenesulfonate and 0.2 parts by weight of sodium carbonate are added again in the reaction. The organic leather tanning agent obtained after the grafting reaction is recorded as 9#.

[0140] Example 10

[0141] This embodiment provides a method for preparing an organic leather tanning agent with covalent tanning properties, and the steps are similar to those of embodiment 3, except that:

[0142] S01, the amounts of raw materials added in the co-condensation reaction are: 12 parts by weight of distilled water, 100 parts by weight of sodium p-aminobenzenesulfonate, 30 parts by weight of phenol, 105 parts by weight of lysine, 25 parts by weight of bisphenol S, 20 parts by weight of salicylic acid, 112 parts by weight of 30% NaOH solution, 104 parts by weight of 37% formaldehyde solution and 5 parts by weight of sodium pyrosulfite. The intermediate obtained by the co-condensation reaction is recorded as 10-a.

[0143] S02, the amounts of raw materials added in the grafting reaction are: 20 parts by weight of distilled water, 19 parts by weight of cyanuric chloride, 4.5 parts by weight of soda ash; 4.3 parts by weight of sodium p-aminobenzenesulfonate and 1 part by weight of sodium carbonate added in the second reaction. The organic leather tanning agent obtained after the grafting reaction is recorded as 10#.

[0144] Embodiment 11

[0145] This embodiment provides a method for preparing an organic leather tanning agent with covalent tanning properties, and the steps are similar to those of Example 2, except that:

[0146] S01. The amounts of raw materials added in the co-condensation reaction are: 90 parts by weight of distilled water, 102 parts by weight of p-aminobenzenesulfonic acid, 42 parts by weight of salicylic acid, 62 parts by weight of urea, 15 parts by weight of 50% sulfuric acid and 121 parts by weight of 37% formaldehyde solution; after completing the co-condensation reaction under acidic conditions, it is neutralized with 78 parts by weight of 30% NaOH solution and post-treated with 6 parts by weight of sodium metabisulfite to obtain an intermediate recorded as 11-a.

[0147] S02, the amounts of raw materials added in the grafting reaction are: 20 parts by weight of distilled water, 22 parts by weight of cyanuric chloride, 6.14 parts by weight of soda ash; 0.79 parts by weight of sodium p-aminobenzenesulfonate and 0.2 parts by weight of sodium carbonate are added again in the reaction. The organic leather tanning agent obtained after the grafting reaction is recorded as 11#.

[0148] Example 12

[0149] This embodiment provides a method for preparing an organic leather tanning agent with covalent tanning properties, and the steps are similar to those of Example 5, except that:

[0150] S01, the addition amount of raw materials in the co-condensation reaction is: 98.8 weight parts of distilled water, 90 weight parts of p-aminobenzenesulfonic acid, 18.2 weight parts of salicylic acid, 32.5 weight parts of bisphenol S, 53.4 weight parts of urea, 13 weight parts of 50% sulfuric acid, 105 weight parts of 37% formaldehyde solution; after the polycondensation reaction is completed under acidic conditions, 67 weight parts of 30% NaOH and 5 weight parts of sodium pyrosulfite are used for post-treatment. The intermediate obtained by the co-condensation reaction is recorded as 12-a.

[0151] S02, the amount of raw materials added in the grafting reaction is: 22 parts by weight of distilled water, 22 parts by weight of cyanuric chloride, 5.7 parts by weight of soda ash; 2.72 parts by weight of sodium p-aminobenzenesulfonate and 0.63 parts by weight of sodium carbonate are added again. The organic leather tanning agent obtained after the grafting reaction is recorded as 12#.

[0152] Comparative Example 1

[0153] This comparative example provides a phenolsulfonic acid formaldehyde condensation product, which is a matrix of a universal synthetic tanning agent and is used as a graft matrix for preparing an active chlorine synthetic tanning agent by modifying TCT. Its structure is:

[0154] The preparation method is as follows:

[0155] In a thermostatic reactor equipped with a thermometer, N2 inlet tube, reflux condenser and mechanical stirring device, add 100g phenol and 116g concentrated sulfuric acid, and carry out phenol sulfonation at 125°C for 8 hours until the sulfonate is soluble in water. Cool the system to 70°C, add 195g water, control the temperature at about 70°C and drop 65g 37% formaldehyde solution. After the formaldehyde is added, keep the temperature at 80°C, continue stirring for 2.5 hours, cool to about 60°C, neutralize with about 170g 40% NaOH solution to pH 6.9, and then cool to room temperature to obtain the phenolsulfonic acid formaldehyde condensation product of the above structure, recorded as 13#, with a solid content of about 43.1%.

[0156] Comparative Example 2

[0157] This comparative example provides an organic leather tanning agent, the structure of which is:

[0158] a'≥50%, b'%≤50%.

[0159] Graft modification step: add 15g of ice water to a clean thermostatic reactor equipped with a thermometer and a mechanical stirring device, place it in a water bath mixed with ice and water, add 15.22g of carefully ground cyanuric chloride powder, start stirring, maintain the temperature at 2 °C and stir rapidly for 30 minutes to obtain a uniformly dispersed cyanuric chloride slurry. Maintain the system temperature below 0-5 °C and slowly add 100g of 13# provided in Comparative Example 1. The mol ratio of phenolic hydroxyl group to TCT in 13# is 2:1. After the addition is completed, slowly drop 11g of 30% NaOH diluted with 30g of water in an aqueous solution within 1 hour, and continue to react at 5 °C for 3 hours after the addition is completed until the reaction of cyanuric chloride is complete (the conversion rate of cyanuric chloride is 99%, including the grafting reaction part with phenolic hydroxyl group and the hydrolysis reaction part with water). After filtering out the hydrolysis by-products insoluble in water, the material is discharged to obtain an organic leather tanning agent with a phenolic hydroxyl group modified by cyanuric chloride as shown above, recorded as 14#, with a solid content of 35.1%, and adjusted to pH 4.2.

[0160] Comparative Example 3

[0161] This comparative example provides an organic leather tanning agent, the structure of which includes a macromolecular tanning agent obtained by reacting TCT with a polymer and a small molecular tanning agent obtained by reacting TCT with a p-aminobenzenesulfonic acid monomer, wherein the structure of the macromolecular tanning agent is:

[0162] a≥25%, b%≤75%.

[0163] The structure of small molecule tanning agent is:

[0164] In this comparative example, the mass percentage of the macromolecular tanning agent is about 72%, and the mass percentage of the small molecule tanning agent is about 18%.

[0165] Graft modification steps: add 60g of ice water to a clean thermostatic reactor equipped with a thermometer and a mechanical stirring device, place it in a water bath mixed with ice and water, start stirring, add 30.45g of carefully ground cyanuric chloride powder, maintain the temperature at 3 and stir rapidly for 30 minutes to obtain a uniformly dispersed cyanuric chloride slurry. Maintain the system temperature at 5 and add 100g of 13# provided in Comparative Example 1 (molar ratio TCT: phenolic hydroxyl = 1:1) slowly drop 16.5g of 30% NaOH and 2g of water diluted aqueous solution within 1 hour, continue to react at below 5 for about 2 hours, and take a sample to test that the conversion rate of cyanuric chloride reaches 75%. While maintaining the system temperature below 4, add cooled aqueous potassium p-aminobenzenesulfonate solution (7.14 g p-aminobenzenesulfonic acid, 10 g water, 4.6 g 50% KOH), and after adding, keep adding 50% KOH 4.6 g dropwise for 5 seconds. Continue the reaction for 2 hours, filter the material, and obtain organic leather tanning agent 15# with a solid content of 35.3%. Adjust the pH to 4.3.

[0166] This comparative example increases the amount of cyanuric chloride added, with the purpose of generating as many macromolecular tanning agents as possible. However, the remaining cyanuric chloride that has not reacted with 13# in comparative example 1 is prone to hydrolysis. In order to avoid TCT hydrolysis, p-aminobenzenesulfonic acid is added to react with the remaining TCT to generate a small molecule tanning agent.

[0167] Test Example 1

[0168] The materials obtained in each step of Examples 1 to 12, the tanning agents provided in Comparative Examples 1 to 3 and the commercially available BTL tanning agent were used to tan the same raw hides in the same manner, and the properties of the leathers were tested to obtain the results shown in Tables 1 and 2.

[0169] Among them, the solid content is tested in an oven at 110°C for 1 hour (ISO3251-2019); the TCT content is calculated based on the amount of cyanuric chloride (TCT) added; the macromolecular tanning agent is an organic leather tanning agent obtained by copolymerization, such as 1# in Example 1; the small molecule tanning agent is an organic leather tanning agent obtained by non-copolymerization, such as the small molecule tanning agent in Comparative Example 3; the content of the macromolecular tanning agent and the small molecule tanning agent is calculated by the amount of raw material added. δTs is the difference in shrinkage temperature before and after tanning of raw hides, indicating the increase in shrinkage temperature after tanning relative to that before tanning. The shrinkage temperature is tested using a MSW-YD4 digital leather shrinkage temperature tester; the grain firmness is tested using sensory evaluation of the finished leather after tanning, with 5 points being the highest and 1 point being the lowest.

[0170] The tanning method is as follows:

[0171] The sheep clothing leather is deashed, softened and pickled according to the conventional process, and the pH of the raw leather is about 7.5 after deashing and softening. The subsequent process measurement standards are based on the quality of the raw leather. The pickled sheep clothing leather is deacidified with 10% salt, 2% NaHCO3 and 3% Na2CO3 to make the pH of the raw leather about 7.5, and then washed thoroughly with water.

[0172] Among them, the tanning process of the tanning agent Xa in the embodiment (X is any integer between 1 and 12), the tanning agent 13# in the comparative example 1 and the BTL tanning agent in the control group includes: the tanning liquid ratio is 50%, the temperature is 35°C, the tanning agent is 10% of the weight of the alkali leather (equivalent to 100% solid content), tanning for 3 hours, and then formic acid is added to gradually adjust the pH to 3.5, the formic acid and pH adjustment time are 3 hours in total, the leather is unloaded from the drum or left to stand overnight before unloading from the drum, the shrinkage temperature of the wet leather is tested and the grain performance is evaluated.

[0173] The tanning process of the tanning agent X# (X is any integer between 1 and 12 and 14 and 15) in the embodiments and comparative examples includes: a tanning liquid ratio of 50%, a temperature of 35°C, a tanning agent of 5% of the weight of the alkali hide (equivalent to 100% solid content), tanning for 3 hours, adding hot water to adjust the temperature to 45°C, continuing tanning for 5 hours, unloading from the drum or leaving it to stand overnight before unloading from the drum, testing the shrinkage temperature of the wet hide and evaluating the grain properties.

[0174] Table 1 Properties of tanning agents

[0175]

[0176]

[0177] Table 2 Properties of tanning agents

[0178]

[0179]

[0180] It can be seen from Table 1 and Table 2 that before the grafting reaction (Xa, X is any integer from 1 to 12), the organic leather tanning agent of Examples 1 to 12 is used to tan raw hides. Even if the amount of the organic leather tanning agent added is greater, the change in its shrinkage temperature is still small. After the grafting reaction (X#, X is any integer from 1 to 12), although the amount of the organic leather tanning agent added is reduced, the shrinkage temperature increases significantly, and the increase difference is much greater than the increase difference before the grafting reaction, indicating that the organic leather tanning agent after active chlorine grafting has a tighter connection with the raw hide, better tanning, and a higher grain tightness score.

[0181] Further detection of the infrared spectra of the tanning agents of Examples 1, 2, 5 and 6 before and after grafting modification, as shown in FIG. Figure 1 and Figure 2 As shown. Figure 1 and Figure 2 It can be seen that the infrared absorption peak increases significantly after modification, indicating that the organic leather tanning agent after grafting modification has more reactive sites, which is conducive to physical or chemical reaction with leather and improves the tanning effect of leather.

[0182] Compared with Example 1, the shrinkage temperature difference of the tanning agents in Comparative Examples 1 to 3 is significantly reduced, which proves that the tanning effect of the tanning agents in the comparative examples is reduced, indicating that the embodiments of the present invention can significantly improve the tanning effect of leather by changing the grafting position of tricyanuric halide.

[0183] Test Example 2

[0184] In order to further test the tanning effect properties of the tanning agent, the leather tanned by the materials obtained in each step of Examples 1, 4 and 9 in Test Example 1, the tanning agents provided in Comparative Examples 1 and 2, and the commercially available BTL tanning agent was detanned, and the properties of the leather were tested to obtain the results shown in Table 3.

[0185] The detanning method comprises: adding 100% normal temperature water to the tanned leather, adjusting the pH value of the system to 6.5-7.0 with soda ash within 1-2 hours, washing out the drum with water, and testing the shrinkage temperature of the leather.

[0186] Table 3 Tanning properties of tanning agents

[0187]

[0188] The δTs in the table are calculated based on the shrinkage temperature of raw hides, that is, the amount by which the tanning agent increases the shrinkage temperature of the leather during the tanning process, and the difference in shrinkage temperature between the leather obtained after detanning and the raw hide, in order to reflect the properties of the tanning effect of the tanning agent.

[0189] It can be seen from Table 3 that the organic leather tanning agents finally obtained in Examples 1, 4 and 9 of the present invention all have good tanning effects, and the shrinkage temperature of the tanned leather obtained after tanning is significantly increased. After detanning, the shrinkage temperature of the leather remains unchanged, and the morphology is the same as after tanning, indicating that the organic leather tanning agent provided by the embodiments of the present invention can maintain its tannability after tanning even after detanning.

[0190] Comparative Example 1 and the commercially available BTL organic leather tanning agent showed certain tannability when tanning raw hides, but after detanning with alkali, the shrinkage temperature of the leather material decreased and the morphology returned to a state close to that of the raw hide, indicating that the grafting position of cyanuric halide also has a significant effect on the tannability of the leather. The organic leather tanning agent of Comparative Example 2 showed a worse morphology of the leather after detanning than before detanning, indicating that the ability to maintain tannability decreased after cyanuric chloride was partially hydrolyzed to form a small molecule tanning agent.

[0191] The reason for the above situation is that the tanning properties of the comparative examples and commercially available samples are essentially hydrogen bonds with relatively weak binding force, which are destroyed by alkaline conditions. However, the organic leather tanning agent provided by the embodiment of the present invention has a change in the grafting position of cyanuric chloride, so the tanning properties between the organic leather tanning agent and the leather are essentially based on covalent bonding that cannot be weakened by weak alkali treatment. Therefore, the leather tanned with the organic leather tanning agent provided by the embodiment of the present invention maintains good tanning properties even after detanning.

[0192] The present invention provides an organic leather tanning agent with covalent tanning properties and a preparation method and application thereof, which has at least the following advantages:

[0193] Since there are many and complex factors that affect the tanning properties of synthetic tanning agents, the size of the tanning agent molecule, the hydrophilicity of the molecule, the content of the hydrophilic group, the content of the tanning group, the solubility of the tanning agent in water, and the permeability all affect the tanning properties of the synthetic tanning agent, the degree of increase in the shrinkage temperature, and the feel and grain properties of the leather. After the hydrophobic cyanuric chloride structure is introduced during the grafting modification process, the synthetic tanning agent still needs to have sufficient hydrophilicity to ensure the good water solubility and permeability of the tanning agent. Therefore, the design of a new synthetic tanning agent with excellent synthetic tanning properties requires comprehensive consideration of the molecular weight of the tanning agent, the tanning group and structural design, the hydrophilicity, the degree of grafting modification, and other aspects. Through the preparation method and the selection and proportion of raw materials, the obtained organic leather tanning agent not only has good hydrophilicity and permeability, but also has good tanning properties.

[0194] The invention provides that the shrinkage temperature of sheepskin rawhide after tanning with a leather tanning agent can be close to 80°C, and the tanned leather has good hand feeling and grain tightness. When the white wet leather obtained after tanning is detanned to a pH of 6.5-7.0, the shrinkage temperature of the leather does not substantially decrease, and the hand feeling and grain characteristics of the leather are not damaged, indicating that the synthetic tanning agent modified with active chlorine is covalently bonded to the leather, and the tanning effect is good and firm and stable. However, the tanning effect of the unmodified general synthetic tanning agent is greatly damaged under the action of external conditions, and is almost close to the rawhide state.

[0195] The organic leather tanning agent provided by the invention has excellent tanning performance, and the tanned leather can be used for further processing to prepare green, environmentally friendly, high-grade and high-quality leather, and has great application potential.

[0196] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. An organic leather tanning agent having covalent tanning properties, characterized in that: The molecular structure of organic leather tanning agent includes A structural unit, B structural unit and C structural unit; The structure of the A structural unit is: The structure of the B structural unit is The structure of the C structural unit is Among them, R1 includes H, -SO3H, -CH2-SO3H, C 1~4 Alkyl, -COOH and Any of; R2 includes H, —OH, and C 1~4 Any of the alkyl groups; R3 includes R4 includes Any of; a is an integer greater than or equal to 0, b is 0 or 1, and a and b cannot be 0 at the same time; c and n are both integers greater than or equal to 1, X is F or Cl, and M is any one of H, alkali metal cation, tertiary amine cation or quaternary ammonium cation.

2. The organic leather tanning agent according to claim 1, characterized in that The general structural formula of the organic leather tanning agent is shown in the following structure: structure:

3. The organic leather tanning agent according to claim 1, characterized in that R1 includes H, -SO3H, -CH2-SO3H, -COOH and Any of; Preferably, R2 comprises H or —OH; Preferably, R3 is Preferably, a is an integer greater than or equal to 0, b is 0 or 1, and a and b cannot be 0 at the same time; c is an integer greater than or equal to 1, X is Cl, and M is H or an alkali metal cation.

4. A method for preparing an organic leather tanning agent as claimed in any one of claims 1 to 3, characterized in that: The method comprises subjecting a p-aminobenzenesulfonic acid raw material, a phenol raw material, an amino raw material and formaldehyde to a co-condensation reaction to obtain an intermediate, wherein the molecular structure of the intermediate includes a polymerization unit shown in structure II, and then subjecting the intermediate to a grafting reaction with tricyanamide; The structure II is:

5. The preparation method according to claim 4, characterized in that: The co-condensation reaction comprises: adding a phenol raw material and / or an amino raw material to a system of a p-aminobenzenesulfonic acid raw material and a pH adjuster, then mixing at a first reaction temperature to obtain a first solution, adding formaldehyde to the first solution, and then heating the solution to perform a co-condensation reaction; Preferably, the pH adjuster is an acid or a base. When the pH adjuster is an acid, the pH of the first solution is ≤3; when the pH adjuster is a base, the pH of the first solution is 9 to 11; Preferably, the method further comprises adding water to the co-polycondensation reaction, and more preferably, the water is deionized water; Preferably, the p-aminobenzenesulfonic acid raw material comprises an aromatic aminosulfonic acid compound or its salt and an aromatic aminocarboxylic acid compound or its salt, and the salt is a sodium salt or a potassium salt; Preferably, the aromatic aminosulfonic acid compound includes any one of p-aminobenzenesulfonic acid, 2,4-diaminobenzenesulfonic acid and p-aminobenzoic acid; Preferably, the aromatic aminocarboxylic acid compound includes any one of aminobenzoic acid, aminophenylacetic acid or aminophenylpropionic acid; Preferably, the phenolic raw material includes at least one of phenol, cresol, ethylphenol, xylenol, bisphenol S, 4,4-dihydroxydiphenyl sulfone, salicylic acid, p-hydroxybenzoic acid, and sulfosalicylic acid; Preferably, the amino raw material includes at least one of urea, carbamate, glycine, lysine and aminoethanesulfonic acid; Preferably, the concentration of formaldehyde is 35-40%; Preferably, the first reaction temperature is 60-70°C; Preferably, after adding formaldehyde, the temperature is raised to 90-95° C. and the reaction is carried out for 3-5 hours.

6. The preparation method according to claim 5, characterized in that: When the pH adjuster is an acid, the weight ratio of the aminobenzenesulfonic acid raw material, the phenol raw material, the amino raw material, water and the pH adjuster is 80-120:30-300:0-62:90-400:5-20; Preferably, the p-aminobenzenesulfonic acid raw material is any one of p-aminobenzenesulfonic acid, 2,4-diaminobenzenesulfonic acid and p-aminobenzoic acid; Preferably, the acid is any one of 50% sulfuric acid, 36.5% concentrated hydrochloric acid or formic acid; Preferably, the weight ratio of the formaldehyde to the p-aminobenzenesulfonic acid raw material is 60-121:80-120.

7. The preparation method according to claim 5, characterized in that: When the pH adjuster is a base, the weight ratio of the aminobenzenesulfonic acid raw material, the phenol raw material, the amino raw material, water and the pH adjuster is 80-120: 0-300: 0-105: 0-400: 5-200; Preferably, the p-aminobenzenesulfonic acid raw material is any one of sodium p-aminobenzenesulfonate, potassium p-aminobenzenesulfonate, sodium 2,4-diaminobenzenesulfonate, sodium p-aminobenzoate and potassium p-aminobenzoate; Preferably, the base is any one of NaOH, Na2CO3 or KOH; Preferably, the weight ratio of the formaldehyde to the p-aminobenzenesulfonic acid raw material is 60-240:80-120.

8. The preparation method according to claim 6 or 7, characterized in that: The method further comprises cooling the system to 48 to 52° C. after the co-polycondensation reaction is completed, adjusting the pH value of the system to 6 to 8, adding sodium metabisulfite to the system and stirring for 20 to 40 minutes; Preferably, the weight ratio of the sodium pyrosulfite to the p-aminobenzenesulfonic acid raw material is 2-30:80-120.

9. The preparation method according to claim 4, characterized in that: The grafting reaction comprises reacting the intermediate with an excess of the cyanuric halide at 0 to 5° C., maintaining the pH of the reaction system at 6 to 8 during the reaction, and adjusting the pH of the system to 4 to 6 after the reaction is completed; Preferably, the molar ratio of the active amino group in the intermediate to the cyanuric halide is 1:0.8-10, more preferably 1:1-1.05; Preferably, the cyanuric halide is cyanuric chloride or cyanuric fluoride, more preferably cyanuric chloride.

10. Use of the organic leather tanning agent as claimed in any one of claims 1 to 3 or the organic leather tanning agent prepared by the preparation method as claimed in any one of claims 4 to 9 in the field of rawhide tanning.

Citation Information

Patent Citations

  • Leather tanning agent and preparation method and application thereof

    CN109628666A

  • Preparation method of modified synthetic tanning agent

    CN113136462A

  • Anhydrous organic leather tanning agent generated based on in-situ reaction as well as preparation method and application of anhydrous organic leather tanning agent

    CN118374642A