Preparation method of high-performance composite diaphragm for alkaline water electrolytic tank

By using thermoplastic resin, hydrophilic inorganic nanoparticles and functional inorganic nanofillers in the composite membrane, combined with adhesive-peeling method and chemical modification, the problem of increased resistance of the composite membrane surface is solved, and high airtightness and The balance of low-plane resistance reduces the energy consumption of hydrogen production by electrolyzing water.

CN118996524APending Publication Date: 2024-11-22TONGJI UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411090346.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

When the existing composite diaphragms pursue high airtightness, the surface resistance increases, resulting in an increase in energy consumption.

Method used

The surface roughness of the support mesh substrate is increased by adhesion-peeling method and active groups are introduced on the surface of the matrix, combining chemical modification and crosslinking agents. , a composite diaphragm with high airtightness and low surface resistance was prepared.

Benefits of technology

The high airtightness and low surface resistance of the composite diaphragm are achieved, the energy consumption of hydrogen production by electrolyzing water is reduced, and the gas purity and electrochemical performance of the diaphragm are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996524A_ABST
    Figure CN118996524A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a high-performance composite diaphragm for an alkaline water electrolytic bath. The method comprises the following steps: dissolving thermoplastic resin in an organic solvent, and adding hydrophilic inorganic nanoparticles and a second type of functional inorganic nanofiller to form a membrane casting solution; the roughness of the substrate of the supporting net is increased through an adhesion-stripping method, and active groups are introduced; tightening a supporting net, and blade-coating the membrane casting solution; after the organic solvent is completely replaced, the composite diaphragm is taken out; and finally cleaning and cutting. The method improves the air tightness and low surface resistance performance of the diaphragm, and is suitable for an efficient alkaline water electrolysis hydrogen production process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a composite diaphragm for an alkaline water electrolytic cell, and in particular to a method for preparing a high-performance composite diaphragm for an alkaline water electrolytic cell. Background Art

[0002] Hydrogen energy has the advantages of abundant sources, green and low-carbon, and wide application, and is of great significance to the strategic transformation of energy. Using renewable energy to produce hydrogen can not only achieve sustainable production of hydrogen, but also solve the problems of spatiotemporal instability and volatility in photovoltaic, wind power and other power generation methods, help large-scale consumption of renewable energy, and achieve large-scale peak load regulation of power grids and cross-seasonal and cross-regional energy storage. It is a bridge connecting renewable energy and users, and can promote the increase of the proportion of renewable energy in primary energy. Therefore, the study of renewable energy water electrolysis hydrogen production technology plays a key role in the current and future energy development.

[0003] As the most mature technology for hydrogen production by electrolysis of water, alkaline water electrolysis has the advantages of simple operation and low cost, and has been commercialized on a large scale. Among them, the diaphragm plays a very important role in the entire water electrolysis system. It prevents the occurrence of safety accidents caused by the cross-permeation of hydrogen and oxygen generated by water electrolysis, and is the core component of the alkaline water electrolyzer. The air tightness of the diaphragm directly determines the purity of hydrogen and oxygen, and affects the production cost of hydrogen production by electrolysis of water. The better the air tightness of the diaphragm, the higher the gas purity, and the higher the pressure that the water electrolysis system can bear, thereby reducing energy consumption and even eliminating the gas compression device. However, while the diaphragm hinders the movement of gas molecules, it also creates resistance to the transmission of hydroxide ions from the cathode to the anode, which is further manifested as an increase in the surface resistance of the diaphragm and increased energy consumption. Therefore, there is a restrictive relationship between the air tightness of the diaphragm and the surface resistance, that is, the better the air tightness, the greater the surface resistance. Therefore, the preparation of high-performance composite diaphragms with high air tightness and low surface resistance is crucial to the performance improvement of alkaline water diaphragms. Summary of the invention

[0004] Aiming at the problem that the air tightness and surface resistance of the existing composite diaphragm are mutually restricted, resulting in a large surface resistance of the composite diaphragm under high air tightness, the present invention proposes a preparation method of a high-performance composite diaphragm with high air tightness and low surface resistance for an alkaline water tank, comprising the following steps:

[0005] (1) dissolving a thermoplastic resin in an organic solvent, adding hydrophilic inorganic nanoparticles and a second type of functional inorganic nanofiller, and mixing them uniformly to obtain a casting solution;

[0006] (2) increasing the surface roughness of the support mesh substrate by an adhesive-peeling method, and then introducing active groups on the substrate surface by chemical modification, copolymerization, cross-linking agents or surfactants;

[0007] (3) The supporting substrate is tightened using a clamp, and then the casting liquid is scraped from bottom to top using scrapers on both sides;

[0008] (4) immersing the coated support mesh substrate in a non-solvent, and taking out the composite diaphragm after the organic solvent is completely replaced;

[0009] (5) The composite diaphragm is cleaned with deionized water, cut into a suitable size, and stored in deionized water.

[0010] Furthermore, the thermoplastic resin includes one or more combinations of polysulfone, polyethersulfone, polyphenylene sulfide, polypropylene, polyetheretherketone, polyimide, and polyetherimide.

[0011] Furthermore, the organic solvent is a combination of one or more of N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, and acetonitrile.

[0012] Furthermore, the hydrophilic inorganic nanoparticles include a combination of one or more of zirconium dioxide, cerium dioxide, titanium dioxide, and barium sulfate.

[0013] Furthermore, the particle size of the hydrophilic inorganic nanoparticles is 10-100 nm.

[0014] Furthermore, the second type of functional inorganic nanofiller is one or more combinations of metal organic frameworks (MOFs), covalent organic frameworks (COFs), and layered double hydroxides (LDHs) with hydroxide ion transport capability.

[0015] Furthermore, the particle size of the second type of functional inorganic nanofiller is 5-100 nm.

[0016] Furthermore, the base material of the support net is PPS; a rubber plate is prepared, and the base material of the rubber plate is glass; a mixture of polyurethane glue and dichloromethane is evenly coated on the rubber plate, wherein the mass ratio of acrylic glue to dichloromethane is 1:10-1:20; a PPS sheet used to prepare the support net is bonded to the rubber plate, wherein the length of the PPS sheet is longer than the rubber plate, so that it has two gripping parts extending outward; after 20-60 seconds of bonding, the PPS sheet is torn off through the gripping parts, because the adhesion of the polyurethane glue to the glass substrate of the rubber plate is greater than the adhesion to PPS, and at the same time, dichloromethane has a dissolving and softening effect on PPS, so that during the tearing process, the polyurethane glue on the rubber plate will stick and peel off part of the surface material of the PPS, thereby forming a roughened surface on the PPS; next, the other side of the PPS sheet is roughened in the same way, and then the PPS sheet is prepared into a PPS support net.

[0017] Furthermore, the active groups include one or more of amine groups, hydroxyl groups, sulfonic acid groups, and carboxyl groups.

[0018] Furthermore, the non-solvent is one or more combinations of deionized water, n-propanol, isopropanol, and ethanol.

[0019] (1) The second type of functional inorganic nanofiller in the present invention not only has a hydrophilic effect, but also facilitates the conduction of hydroxide ions. By introducing the second type of functional inorganic nanofiller, a hydrogen bond network is constructed in the membrane, a new hydroxide ion transport mechanism (such as the Grotthuss mechanism) is introduced, the hydroxide ion transfer process in the membrane is strengthened, and the influence of the membrane pore structure on the surface resistance is greatly reduced.

[0020] (2) The second type of functional inorganic nanofillers in the present invention are all in two-dimensional form to achieve controllable regulation of the pore structure of the composite diaphragm. The second type of functional inorganic nanofillers of appropriate size are combined with spherical inorganic nanoparticles of specific particle size to form different stacking structures, which provides a new idea for regulating the pore size distribution of the composite diaphragm and can further improve the air tightness of the composite diaphragm.

[0021] (3) The roughening treatment of the support mesh substrate bonding-peeling method proposed in the present invention can increase the surface roughness of the support mesh substrate, increase the effective contact area between the coating and the support mesh substrate, and improve the bonding strength. It is not limited by materials and has universality.

[0022] (4) The present invention performs surface modification on the support mesh substrate, introduces active groups, and improves the surface energy of the support mesh substrate material, making its surface easier to interact and adhere with other materials, improving compatibility, and enhancing the adhesion between the coating and the support mesh substrate.

[0023] The active groups introduced in the present invention are not only beneficial to improving the stability of the ultra-thin composite diaphragm, but also increase the hydrophilicity of the support mesh substrate, reduce the surface resistance of the composite diaphragm, and reduce the energy consumption of water electrolysis.

[0024] The concept, specific structure and technical effects of the present invention will be further described below in conjunction with the accompanying drawings to fully understand the purpose, characteristics and effects of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a process flow chart of the present invention;

[0026] Figure 2 is a schematic diagram of a rubber plate substrate in a preferred embodiment of the present invention;

[0027] Figure 3 is a schematic diagram of a rubber plate substrate after being coated with glue in a preferred embodiment of the present invention;

[0028] Figure 4It is a schematic diagram of bonding a PPS sheet used for preparing a support mesh to a rubber plate in a preferred embodiment of the present invention;

[0029] Figure 5 It is a schematic diagram of tearing a PPS sheet off a rubber plate to form a roughened surface on the surface in a preferred embodiment of the present invention;

[0030] Figure 6 is a cross-sectional SEM image of the composite diaphragm prepared in Example 1 of the present invention;

[0031] Figure 7 and Figure 8 The graphs are comparative diagrams of Examples 1-4 and the composite diaphragm without replacing the second type of functional inorganic nanofiller in terms of air tightness (bubble point pressure), surface resistance and actual electrochemical performance (polarization curve) in the electrolytic cell. DETAILED DESCRIPTION

[0032] The following describes several preferred embodiments of the present invention with reference to the drawings in the specification, so that the technical content is clearer and easier to understand. The present invention can be embodied in many different forms of embodiments, and the protection scope of the present invention is not limited to the embodiments mentioned in the text.

[0033] See also Figure 1 The present invention provides a method for preparing a high-performance composite diaphragm for an alkaline water tank, and the specific method steps include:

[0034] (1) Preparation of casting solution

[0035] The thermoplastic resin is dissolved in an organic solvent, and then hydrophilic inorganic nanoparticles and a second type of functional inorganic nanofiller are added, and the mixture is evenly mixed by mechanical stirring or ball milling, ultrasound or other dispersion methods to obtain a casting solution.

[0036] (2) Roughening of the support mesh base

[0037] In order to achieve the purpose of low surface resistance, the composite diaphragm needs to be as thin as possible. In addition to being limited by the size of the scraping, the thickness of the composite diaphragm mainly depends on the thickness of the support mesh substrate that provides mechanical strength. That is, a thinner support mesh substrate is required to prepare a thinner composite diaphragm. However, in order to ensure the mechanical strength of the substrate, the thickness is reduced, the mesh number of the substrate is increased, and the contact area of ​​the coating scraped on the left and right sides is reduced, resulting in the stability of the composite diaphragm mainly depending on the adhesion between the coating and the support mesh substrate. The adhesion between the coating and the support mesh substrate is much smaller than the interaction force between the coatings. Therefore, when the mesh number of the support mesh substrate exceeds 150, the stability of the composite diaphragm is poor, and the coating on both sides often falls off.

[0038] The present invention increases the surface roughness of the support mesh substrate by an adhesive-peeling method, and then introduces active groups on the substrate surface by chemical modification, copolymerization, crosslinking agent or surfactant.

[0039] (3) Coating of casting solution

[0040] The dry and clean support substrate is tightened with a clamp, and then the casting liquid is scraped symmetrically from bottom to top with scrapers on both sides. The thickness of the composite diaphragm can be freely adjusted by selecting support substrates of different thicknesses or scrapers of different specifications according to specific needs.

[0041] (4) Phase transformation

[0042] At 25° C., the double-sided coated support substrate was immersed in a non-solvent, and the non-solvent was changed every half an hour. After the organic solvent was completely replaced, the composite separator was taken out.

[0043] (5) Clean and store

[0044] The composite diaphragm was cleaned with deionized water, cut into appropriate sizes, and stored in deionized water.

[0045] In step (1), the thermoplastic resin includes one or more combinations of polysulfone, polyethersulfone, polyphenylene sulfide, polypropylene, polyetheretherketone, polyimide, and polyetherimide.

[0046] In step (1), the organic solvent is a combination of one or more of N-methyl-2-pyrrolidone, dimethyl sulfoxide, N,N-dimethylformamide, formamide, and N,N-dimethylacetamide.

[0047] In step (1), the hydrophilic inorganic nanoparticles include a combination of one or more of zirconium dioxide, cerium dioxide, titanium dioxide, and barium sulfate, and have a particle size of 10-100 nm.

[0048] In step (1), the second type of functional inorganic nanofiller is one or more combinations of metal organic frameworks (MOFs), covalent organic frameworks (COFs) or layered double hydroxides (LDHs) with hydroxide ion transport capability, and has a particle size of 5-100 nm.

[0049] In step (2), the support substrate is a mesh, a porous membrane, a non-woven fabric, a woven fabric, or other forms of composite fabric, and the material includes one or more combinations of polyphenylene sulfide, polyethylene, polypropylene, polytetrafluoroethylene, polyetheretherketone, and polyimide; see Figure 2 In a preferred embodiment, the surface roughened support mesh is prepared as follows: the support mesh base material is PPS; prepare a rubber plate 1, the rubber plate base material is glass; see Figure 3, a mixture 2 of polyurethane glue and dichloromethane is evenly coated on the rubber plate 1, wherein the mass ratio of acrylic glue to dichloromethane is 1:10-1:20; see Figure 4 , the PPS sheet 3 used to prepare the support mesh is bonded to the rubber plate 1, the length of the PPS sheet 3 is longer than the rubber plate 1, so that it has two gripping parts 3 and 4 extending outward; see Figure 5 After 20-60 seconds of pasting, the PPS sheet is torn off by the gripping parts 3 and 4. Since the adhesion of the polyurethane adhesive to the glass substrate of the adhesive sheet is greater than the adhesion to PPS, it will remain on the glass substrate during tearing. At the same time, dichloromethane has a dissolving and softening effect on PPS. In this way, during the tearing process, the polyurethane adhesive on the adhesive sheet will stick to and peel off part of the surface material of PPS, thereby forming a roughened surface 6 on the PPS. Next, the other side of the PPS sheet 3 is roughened in the same way, and then the PPS sheet is prepared into a PPS support network.

[0050] In step (2), the active group includes one or more of an amino group, a hydroxyl group, a sulfonic acid group, and a carboxyl group;

[0051] In step (4), the non-solvent is one or more of deionized water, n-propanol, isopropanol, and ethanol.

[0052] Example 1

[0053] At normal pressure and room temperature, 15 g of polysulfone is placed in 85 g of N-methyl-2-pyrrolidone (NMP) and mechanically stirred until the polysulfone is completely dissolved, and then 63.75 g of zirconium oxide with a particle size of 10-100 nm and 21.25 g of NiFe-LDH are added in batches, and the mixture is mechanically stirred and dispersed at 2000 rpm for 66 hours, and a casting solution is obtained after standing and degassing; a surface-roughened PPS mesh is fixed between two scrapers with a gap of 300 μm, and the casting solution is evenly applied from bottom to top; the coated PPS mesh is immersed in deionized water at 25° C. for phase inversion, and the water is changed every half an hour until the concentration of NMP in the deionized water remains unchanged, so as to obtain a composite diaphragm; the composite diaphragm is rinsed with deionized water, and it is cut into a suitable size and stored in deionized water.

[0054] Figure 6 This is a cross-sectional SEM image of the composite membrane prepared in Example 1. It can be seen that the hydrophilic zirconium oxide and NiFe-LDH are evenly distributed in the composite membrane, and together with the polysulfone, they form a pore structure with fine and uniform pore size, thereby ensuring the airtightness of the composite membrane.

[0055] In Example 2-4, the implementation method is the same as that in Example 1, except that only the parameters are changed.

[0056] Figure 7 and Figure 8Comparison diagrams of Examples 1-4 and the composite diaphragm without replacing the second type of functional inorganic nanofiller in terms of air tightness (bubble point pressure), surface resistance and actual electrochemical performance (polarization curve) in the electrolytic cell are shown respectively. It can be seen that replacing the hydrophilic inorganic particles with the second type of functional inorganic nanofiller not only improves the air tightness of the composite diaphragm, but also significantly reduces the surface resistance and improves the electrochemical performance, proving that the second type of functional inorganic nanofiller greatly improves the conductivity of hydroxide ions in the membrane, realizes the decoupling of the air tightness and surface resistance of the composite diaphragm, and successfully prepares a high-performance composite diaphragm with high air tightness and low surface resistance for alkaline water electrolyzer.

[0057] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A method for preparing a high-performance composite diaphragm for an alkaline water tank, It is characterized in that The following steps are involved: (1) dissolving a thermoplastic resin in an organic solvent, adding hydrophilic inorganic nanoparticles and a second type of functional inorganic nanofiller, and mixing them uniformly to obtain a casting solution; (2) increasing the surface roughness of the support mesh substrate by an adhesive-peeling method, and then introducing active groups on the substrate surface by chemical modification, copolymerization, cross-linking agents or surfactants; (3) The supporting substrate is tightened using a clamp, and then the casting liquid is scraped from bottom to top using scrapers on both sides; (4) immersing the coated support mesh substrate in a non-solvent, and taking out the composite diaphragm after the organic solvent is completely replaced; (5) The composite diaphragm is cleaned with deionized water, cut into a suitable size, and stored in deionized water.

2. The method for preparing the high-performance composite diaphragm for alkaline water electrolyzer according to claim 1, in, The thermoplastic resin includes one or more combinations of polysulfone, polyethersulfone, polyphenylene sulfide, polypropylene, polyetheretherketone, polyimide, and polyetherimide.

3. The method for preparing the high-performance composite diaphragm for alkaline water electrolyzer according to claim 1, in, The organic solvent is a combination of one or more of N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide and acetonitrile.

4. The method for preparing the high-performance composite diaphragm for alkaline water electrolyzer according to claim 1, in, The hydrophilic inorganic nanoparticles include one or more of zirconium dioxide, cerium dioxide, titanium dioxide and barium sulfate.

5. The method for preparing the high-performance composite diaphragm for alkaline water electrolyzer according to claim 4, in, The particle size of the hydrophilic inorganic nanoparticles is 10-100 nm.

6. The method for preparing the high-performance composite diaphragm for alkaline water electrolyzer according to claim 1, in, The second type of functional inorganic nanofillers is one or more combinations of metal organic frameworks (MOFs), covalent organic frameworks (COFs), and layered double hydroxides (LDHs) with hydroxide ion transport capabilities.

7. The method for preparing the high-performance composite diaphragm for alkaline water electrolyzer according to claim 6, in, The particle size of the second type of functional inorganic nanofillers is 5-100 nm.

8. The method for preparing the high-performance composite diaphragm for alkaline water electrolyzer according to claim 1, in, The base material of the support net is PPS; a rubber plate is prepared, and the base material of the rubber plate is glass; a mixture of polyurethane glue and dichloromethane is evenly coated on the rubber plate, wherein the mass ratio of acrylic glue to dichloromethane is 1:10-1:20; a PPS sheet used to prepare the support net is bonded to the rubber plate, wherein the length of the PPS sheet is longer than the rubber plate, so that it has two gripping parts extending outward; after 20-60 seconds of bonding, the PPS sheet is torn off through the gripping parts, because the adhesion of the polyurethane glue to the glass substrate of the rubber plate is greater than the adhesion to PPS, and at the same time, dichloromethane has a dissolving and softening effect on PPS, so that during the tearing process, the polyurethane glue on the rubber plate will stick and peel off part of the surface material of the PPS, thereby forming a roughened surface on the PPS; next, the other side of the PPS sheet is roughened in the same way, and then the PPS sheet is prepared into a PPS support net.

9. The method for preparing the high-performance composite diaphragm for alkaline water electrolyzer according to claim 1, in, The active groups include one or more of amine groups, hydroxyl groups, sulfonic acid groups, and carboxyl groups.

10. The method for preparing the high-performance composite diaphragm for alkaline water electrolyzer according to claim 1, in, The non-solvent is one or more combinations of deionized water, n-propanol, isopropanol, and ethanol.

Citation Information

Cited By

  • Solid electrolyte membrane for hydrogen production by alkaline electrolyzed water and preparation method and application thereof

    CN120060923A

  • Composite diaphragm for alkaline electrolyzed water and preparation method of composite diaphragm

    CN121228289A