Photovoltaic module

By applying film tape and modified coating on the organic light-transmitting back plate of double-sided single-glass photovoltaic module, the bubble and delamination problems during aging are solved, the power and reflectivity of the photovoltaic module are improved, and the adhesion is enhanced. Extend the service life of the components.

CN119008749AActive Publication Date: 2024-11-22JINKO SOLAR CO LTD +1

Patent Information

Application Number
CN202411215757.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-22
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

The gap film of the double-sided single-glass photovoltaic module has an inadequate aging problem when it is bonded on the organic light-transmitting back plate, which is prone to bubbles and delamination, resulting in a degradation of performance.

Method used

The film belt is attached to the organic light-transmitting back plate. The film belt includes a modified EVA layer, with a cross-linking degree of 65%~85%, a VA content of 28%~33% and a modified coating is formed on the back plate, with a rough surface. The degree is 1.1μm±0.1μm to improve cohesion strength and bonding force and reduce bubble occurrence.

Benefits of technology

The power and reflectivity of the photovoltaic module are improved, the adhesion between the membrane belt and the back plate is enhanced, the aging resistance of the module is extended, and the delamination problem is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008749A_ABST
    Figure CN119008749A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of photovoltaic technology, in particular to a photovoltaic module. The photovoltaic module comprises a front cover plate, a plurality of battery pieces, a film belt and an organic light-transmitting back plate, the battery pieces are arranged between the front cover plate and the organic light-transmitting back plate at intervals, and the film belt is located on the side, close to the battery pieces, of the organic light-transmitting back plate; the film belt comprises a modified EVA layer, the content of VA in the modified EVA layer is 28 wt%-33 wt%, and the modified EVA layer is in contact with the organic light-transmitting back plate; the surface roughness of the side, making contact with the modified EVA, of the organic light-transmitting backboard is 1.1 [mu] m + / -0.1 [mu] m. Bubbles generated between the film belt and the organic light-transmitting back plate can be effectively reduced, and the delamination problem is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of photovoltaic technology, and in particular to a photovoltaic module. Background Art

[0002] Photovoltaic modules can be divided into bifacial and single-sided modules according to whether the back side is light-transmissive. Bifacial modules refer to modules with both sides of the cell set as light-transmissive panels, and the back side can also absorb the reflected light from the ground and convert sunlight into electricity; single-sided modules refer to modules with the back side of the cell set as non-transparent panels, and can only collect sunlight from the front side and convert it into electricity. Compared with single-sided modules, bifacial modules have higher power generation gain per watt.

[0003] According to the different back packaging of the battery cells, bifacial photovoltaic modules can be divided into bifacial double-glass photovoltaic modules and bifacial single-glass photovoltaic modules. Bifacial double-glass photovoltaic modules refer to modules with glass panels on both the front and back of the battery cells, while bifacial single-glass photovoltaic modules refer to modules with glass panels on the front and organic light-transmitting back panels on the back.

[0004] Photovoltaic module gap film technology refers to adding specific film materials in the gap between photovoltaic cells to improve the photoelectric conversion efficiency of solar cells. The gap film can improve the utilization rate of sunlight by reflecting and absorbing the light in the gap without affecting the normal operation of the cell, thereby improving the overall performance of the photovoltaic module. At present, the gap film of the double-sided double-glass photovoltaic module is mainly formed by applying a film tape to the glass or screen printing a glaze containing titanium dioxide (TiO2) on the glass, while the gap film of the double-sided single-glass photovoltaic module can only be formed by screen printing a glaze containing titanium dioxide (TiO2) on the organic transparent backplane, because if the film tape bonded to the glass is bonded to the organic transparent backplane, there is a problem of not being resistant to aging. During the aging process, bubbles are prone to appear between the film tape and the organic transparent backplane, which leads to delamination problems. Summary of the invention

[0005] Based on this, the first aspect of the present application provides a photovoltaic module, and its technical solution is as follows:

[0006] A photovoltaic module comprises a front cover, a plurality of cells, a film strip and an organic light-transmitting backplane, wherein the plurality of cells are arranged between the front cover and the organic light-transmitting backplane at intervals, and the film strip is located on a side of the organic light-transmitting backplane close to the cells;

[0007] The film tape includes a modified EVA layer, the organic light-transmitting backplane includes a modified coating, the modified EVA layer is in contact with the modified coating, the crosslinking degree of the modified EVA layer is 65%~85%, the VA content is 28wt%~33wt%, and the surface roughness of the modified coating is 1.1μm±0.1μm.

[0008] Compared with the traditional solution, this application has the following beneficial effects:

[0009] The present application applies a film tape to an organic light-transmitting backplane, which is beneficial to improving the power and reflectivity of photovoltaic modules compared to screen-printing a glaze containing titanium dioxide (TiO2) on glass. In order to ensure the feasibility of backplane film application, the film tape and the organic light-transmitting backplane are modified at the same time, wherein the film tape includes a modified EVA layer, and the organic light-transmitting backplane includes a modified coating. The crosslinking degree of the modified EVA layer is 65%~85%, the VA content is 28wt%~33wt%, and the surface roughness of the modified coating is 1.1μm±0.1μm. Through the above-mentioned modification, on the one hand, the cohesive strength and surface polarity of the film tape itself are improved, and on the other hand, the surface roughness is improved, and the adhesion of the contact surface is increased. During the aging process, the bubbles generated between the film tape and the organic light-transmitting backplane can be effectively reduced, and the delamination problem can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] In order to more clearly illustrate the technical solutions in the embodiments of the present application and to more completely understand the present application and its beneficial effects, the following is a brief introduction to the drawings required for the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.

[0011] Figure 1 It is a schematic diagram of the structure of a traditional double-sided single-wave photovoltaic module;

[0012] Figure 2 Schematic diagram of bubbles appearing between the film strip and the organic light-transmitting backplane;

[0013] Figure 3 It is a schematic structural diagram of a double-sided single-wave photovoltaic module according to one embodiment;

[0014] Figure 4 is a schematic structural diagram of a membrane tape according to an embodiment;

[0015] Figure 5 A schematic structural diagram of a membrane tape according to another embodiment;

[0016] Figure 6 Schematic diagram of the structure of an organic light-transmitting backplane according to one embodiment. DETAILED DESCRIPTION

[0017] The present application will be further described in detail below in conjunction with specific embodiments. The present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thoroughly understood.

[0018] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0019] the term

[0020] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:

[0021] In the present application, "plurality", "multiple", "multiple times", "plurality", etc., unless otherwise specified, refer to a number greater than 2 or equal to 2. For example, "one or more" means one or greater than or equal to two.

[0022] In the present application, “several” means at least one, such as one, two, etc., unless otherwise clearly defined.

[0023] In this application, "optionally", "optional" and "optional" refer to optional, that is, to any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.

[0024] In this application, in the "first aspect", "second aspect", "third aspect", "fourth aspect", etc., the terms "first", "second", "third", "fourth", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0025] In the present application, when referring to a numerical interval (i.e., a numerical range), unless otherwise specified, the optional numerical distribution within the above numerical interval is deemed to be continuous and includes the two numerical endpoints of the numerical range (i.e., the minimum value and the maximum value), and every numerical value between the two numerical endpoints.

[0026] The temperature parameters in this application, unless otherwise specified, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.

[0027] In the present application, %(w / w) and wt% both represent weight percentage, %(v / v) refers to volume percentage, and %(w / v) refers to mass volume percentage.

[0028] At present, the gap film of double-sided double-glass photovoltaic modules is mainly formed by applying a film tape to the glass or screen-printing a glaze containing titanium dioxide (TiO2) on the glass, while the gap film of double-sided single-glass photovoltaic modules can only be formed by screen-printing a glaze containing titanium dioxide (TiO2) on the organic transparent backplane. Please refer to Figure 1 , is a schematic diagram of the structure of a conventional bifacial single-wave photovoltaic module 100, comprising a front cover plate 11, a plurality of cells 12, a glaze layer 13 and an organic light-transmitting backplane 14, wherein the plurality of cells 12 are arranged at intervals between the front cover plate 11 and the organic light-transmitting backplane 14, the glaze layer 13 is located on the side of the organic light-transmitting backplane 14 close to the cells 12, and the front cover plate 11, the plurality of cells 12, the glaze layer 13 and the organic light-transmitting backplane 14 are bonded by a transparent adhesive film. The glaze layer 13 is formed by printing a glaze containing titanium dioxide (TiO2), which has a reflective effect on light. It can improve the utilization rate of sunlight by reflecting and absorbing the light in the gap between the cells without affecting the normal operation of the cells, thereby improving the overall performance of the photovoltaic module. However, the surface of the glaze layer is rough and uneven, and diffusely reflects the incident light. Compared with the film tape that fully reflects the incident light, the utilization rate of diffusely reflecting the incident light is insufficient. However, it is currently impossible to form a gap film on the organic light-transmitting backplane film tape, because if the film tape bonded to the glass is bonded to the organic light-transmitting backplane, there is a problem of poor aging resistance. During the aging process, bubbles are easily formed between the film tape 15 and the organic light-transmitting backplane 14. Please refer to Figure 2 , which leads to the problem of delamination.

[0029] This application provides a photovoltaic module, see Figure 3 In one embodiment, the photovoltaic module 200 includes a front cover plate 21, a plurality of cells 22, a film strip 23 and an organic light-transmitting backplane 24, wherein the plurality of cells 22 are arranged at intervals between the front cover plate 21 and the organic light-transmitting backplane 24, and the film strip 23 is located on a side of the organic light-transmitting backplane 24 close to the cells 22, wherein the front cover plate 21, the plurality of cells 22, the film strip 23 and the organic light-transmitting backplane 24 can be bonded by a transparent adhesive film. In this embodiment, the film strip 23 is attached to the organic light-transmitting backplane 24. Compared with printing a glaze containing titanium dioxide (TiO2) on the organic light-transmitting backplane 24 to form a glaze layer, the film strip 23 can fully reflect the incident light, thereby improving the light utilization rate, which is beneficial to improving the power and reflectivity of the photovoltaic module.

[0030] In order to solve the problem of bubbles easily appearing between the film tape 23 and the organic light-transmitting backplane 24, the film tape is modified. After the modification, the film tape 23 includes a modified EVA layer, wherein the crosslinking degree of the modified EVA layer is 65%~85%, and the VA (vinyl acetate) content is 28wt%~33wt%. The crosslinking degree of the modified EVA layer includes but is not limited to 65%, 70%, 75%, 80%, and 85%. The VA content includes but is not limited to 28wt%, 29wt%, 30wt%, 31wt%, 32wt%, and 33wt%. The crosslinking degree and VA content of the modified EVA layer can be adjusted to be within the above range. Controlling the crosslinking degree within the range of 65%~85% is conducive to improving the cohesive strength of the film tape itself, thereby improving the bonding force. Controlling the VA content within the range of 28wt%~33wt% is conducive to increasing the surface polarity of the film tape and improving the bonding force between the surface of the film tape and the surface of the organic light-transmitting backplane 24.

[0031] The modified EVA layer can be obtained by modifying the traditional EVA layer by adding an auxiliary agent to the traditional EVA layer formula or increasing the content of vinyl acetate monomer. Optionally, the raw materials of the modified EVA layer include a main resin and an auxiliary agent, the main resin includes ethylene monomer and vinyl acetate monomer, and the auxiliary agent includes one or more of a coupling agent and a cross-linking agent. By controlling the amount of the auxiliary agent and the polar material (VA), the cross-linking degree and VA content of the modified EVA layer can be controlled.

[0032] Optionally, the thickness of the modified EVA layer is 1 μm to 100 μm. For example, the thickness of the modified EVA layer is 1 μm, 20 μm, 50 μm, 80 μm, or 100 μm.

[0033] See also Figure 4 In this embodiment, the film strip 23 includes a modified EVA layer 231, a PET support layer 232, a concavo-convex structure 233, an insulating layer 234 and an aluminum reflective layer 235. The modified EVA layer 231 is as described above. The PET support layer 232 is located on the side of the modified EVA layer 231 away from the organic light-transmitting backplane 14, the concavo-convex structure 233 is located on the side of the PET support layer 232 away from the modified EVA layer 231, the insulating layer 234 is located on the side of the concavo-convex structure 233 away from the PET support layer 232, and the aluminum reflective layer 235 is located on the side of the insulating layer 234 away from the concavo-convex structure 233.

[0034] In this embodiment, the reflective layer is an aluminum reflective layer. The reflectivity of metal aluminum (≥85%) is higher than the reflectivity of the glaze layer (≥75%), and the light utilization rate is higher.

[0035] Optionally, the position of the film tape corresponds to the gap between two adjacent battery cells, or multiple battery cells are connected in series to form multiple battery strings, and the position of the film tape corresponds to the gap between two adjacent battery strings. Optionally, the width of the film tape is 2 mm to 6 mm.

[0036] This embodiment does not limit the structure of the battery cell. The types of battery cells include but are not limited to Passivated Emitter Rear Cell (PERC), Tunnel Oxide Passivated Contact (TOPCon), Heterojunction with Intrinsic Thin-film (HJT), Interdigitated Back Contact (IBC), perovskite cells, etc.

[0037] For PERC cells, along the thickness direction, PERC cells include the front surface metal silver electrode, the front surface silicon nitride passivation layer, the phosphorus layer emitter, the P-type base silicon layer, the local aluminum back field, the metal aluminum back electrode, and the back passivation layer (Al2O3 / SiNx). PERC cells use a passivation film to passivate the back, replacing the full aluminum back field, enhancing the internal back reflection of light in the silicon base, reducing the recombination rate on the back, and increasing the efficiency of the cell by 0.5%-1%.

[0038] For TOPCon cells, along the thickness direction, TOPCon cells include metal silver electrodes, front surface silicon nitride passivation layers, boron-doped emitters, N-type base silicon layers, diffused doping layers, ultra-thin silicon oxide, doped polysilicon, silicon nitride, and metal silver electrodes. The back of the cell is composed of an ultra-thin silicon oxide layer (1nm~2nm) and a phosphorus-doped microcrystalline amorphous mixed Si film, which together form a passivation contact structure. This structure can block the recombination of minority carrier holes and increase the open circuit voltage and short circuit current of the cell. The ultra-thin oxide layer allows majority electrons to tunnel into the polysilicon layer while blocking the recombination of minority carrier holes. The good passivation effect of ultra-thin silicon oxide and heavily doped silicon film causes the energy band on the silicon wafer surface to bend, thereby forming a field passivation effect, greatly increasing the probability of electron tunneling, and reducing the contact resistance, which increases the open circuit voltage and short circuit current of the cell, thereby improving the cell conversion efficiency.

[0039] For HJT cells, along the thickness direction, the HJT cells include a front low-temperature silver electrode, a front conductive film, an N-type amorphous silicon film, an intrinsic amorphous silicon film, an N-type base silicon layer, an intrinsic amorphous silicon film, a P-type amorphous silicon film, a back conductive film, and a back low-temperature silver electrode.

[0040] For IBC cells, along the thickness direction, IBC cells include silicon nitride anti-layer, N+ front surface field, N-type base silicon layer, P+ emitter, N+ back field, aluminum oxide passivation layer, silicon nitride anti-reflection layer, and metal silver electrode. IBC cells use ion implantation technology to obtain P and N regions with good uniformity and precisely controllable junction depth. There is no grid line blocking on the front of the cell, which can eliminate the shading current loss of the metal electrode and achieve the maximum utilization of incident photons. The short-circuit current can be increased by about 7% compared with conventional solar cells; due to the back contact structure, there is no need to consider the grid line blocking problem, and the grid line ratio can be appropriately widened, thereby reducing the series resistance and having a high fill factor; the surface passivation and surface light trapping structure can be optimized to obtain a lower front surface recombination rate and surface reflection.

[0041] For perovskite cells, along the thickness direction, the perovskite cell includes substrate material, conductive film, electron transport layer (titanium dioxide), perovskite absorption layer (hole transport layer), and metal cathode. Perovskite materials have a high light absorption coefficient and a long carrier diffusion distance. After the photons absorbed by the perovskite material are converted into electrons, they are easily collected by the electrode with low loss, so they can generate higher photoelectric voltage and current, making perovskite show higher photoelectric conversion efficiency.

[0042] Generally, to ensure that there is no light leakage, the width of the glaze layer formed on the organic transparent backplane is greater than the gap between two adjacent battery cells, so that more incident light from the back is blocked. In this embodiment, the position and size of the film tape corresponds to the gap between two adjacent battery cells. The width of the film tape can be set according to the gap between two adjacent battery cells (0~2mm). Compared with the traditional glaze layer, the width of the film tape can be narrowed and the double-sided rate can be improved. In other embodiments, multiple battery cells are connected in series to form multiple battery strings, and the position and size of the film tape correspond to the gap between two adjacent battery strings.

[0043] In another embodiment, see Figure 5The film strip 33 includes a modified EVA layer 331, an EVA layer 336, a PET support layer 332, a concavo-convex structure 333, an insulating layer 334 and an aluminum reflective layer 335. The crosslinking degree of the modified EVA layer 331 is 65% to 85%, and the VA content is 28wt% to 33wt%. The PET support layer 332 is located on the side of the modified EVA layer 331 away from the organic light-transmitting backplane 14, and the EVA layer 336 is located between the modified EVA layer 331 and the PET support layer 332. The concavo-convex structure 333 is located on the side of the PET support layer 332 away from the modified EVA layer 331, the insulating layer 334 is located on the side of the concavo-convex structure 333 away from the PET support layer 332, and the aluminum reflective layer 335 is located on the side of the insulating layer 334 away from the concavo-convex structure 333. In this embodiment, a part of the EVA layer is modified.

[0044] Optionally, the film tape has a thickness of 50 μm to 150 μm, including but not limited to 50 μm, 75 μm, 100 μm, and 150 μm.

[0045] In order to solve the problem of bubbles easily appearing between the film tape 23 and the organic light-transmitting backplane 24, the present application not only modifies the film tape 23, but also modifies the organic light-transmitting backplane 24 in conjunction with the modification of the film tape 23. After the modification, the organic light-transmitting backplane 24 includes a modified coating, and the surface roughness of the modified coating is 1.1μm±0.1μm. At this time, the modified coating of the organic light-transmitting backplane 24 is in contact with the modified EVA layer of the film tape 23. The surface roughness of the modified coating is 1.1μm±0.1μm, which is conducive to increasing the adhesion of the contact surface between the organic light-transmitting backplane 24 and the film tape 23. By improving the film tape 23 and the organic light-transmitting backplane 24 at the same time, not only the adhesion between the two is improved under normal conditions, but more importantly, the adhesion between the two can be maintained during the aging process, which can effectively reduce the bubbles generated between the film tape and the organic light-transmitting backplane and improve the delamination problem between the film tape and the organic light-transmitting backplane.

[0046] Optionally, the modified coating contains SiO2 particles. By adding SiO2 particles to the coating of the traditional coating, the roughness of the modified coating can be improved without affecting the reliability and transmittance of the organic transparent backplane. Before and after the addition of SiO2 particles, the roughness of the modified coating can be increased from the initial 0.55μm±0.1μm to 1.1μm±0.1μm.

[0047] Optionally, the average particle size of the SiO2 particles is 5 μm±1 μm.

[0048] Optionally, the SiO2 particles account for 5%±1% by mass in the modified coating.

[0049] Optionally, the coating of the modified coating includes a main resin, a functional additive and the SiO2 particles, the main resin includes a fluorocarbon resin and an acrylic resin, and the functional additive includes one or more of an ultraviolet absorber, a light stabilizer, an anti-hydrolysis agent, a leveling agent and a dispersant.

[0050] Optionally, the modified coating has a thickness of 50 μm to 180 μm, including but not limited to 50 μm, 75 μm, 100 μm, 150 μm, and 180 μm.

[0051] See also Figure 6 In this embodiment, the organic light-transmitting backplane 24 includes a modified coating 241, an organic matrix 242 and a protective coating 243, wherein the modified coating is as described above. The organic matrix 242 is located on the side of the modified coating 241 away from the film strip 23, and the protective coating 243 is located on the side of the organic matrix 242 away from the modified coating 241.

[0052] Alternatively, the material of the organic matrix may be PET.

[0053] Optionally, the coating of the protective coating includes a main resin and a functional additive, the main resin includes a fluorocarbon resin and an acrylic resin, and the functional additive includes one or more of an ultraviolet absorber, a light stabilizer, an anti-hydrolysis agent, a leveling agent and a dispersant.

[0054] This embodiment of the invention is to apply a film tape to the organic light-transmitting backplane, which is more conducive to improving the power and reflectivity of photovoltaic modules than screen-printing a glaze containing titanium dioxide (TiO2) on glass. In order to ensure the feasibility of backplane film application, the film tape and the organic light-transmitting backplane are modified at the same time, wherein the film tape includes a modified EVA layer, and the organic light-transmitting backplane includes a modified coating. The crosslinking degree of the modified EVA layer is 65% to 85%, the VA content is 28wt% to 33wt%, and the surface roughness of the modified coating is 1.1μm±0.1μm. Through the above-mentioned modification, on the one hand, the cohesive strength and surface polarity of the film tape itself are improved, and on the other hand, the surface roughness is improved, and the adhesion of the contact surface is increased. During the aging process, the bubbles generated between the film tape and the organic light-transmitting backplane can be effectively reduced, and the delamination problem can be improved.

[0055] The following is further described in conjunction with specific embodiments and comparative examples. The raw materials involved in the following specific embodiments and comparative examples, unless otherwise specified, can all be commercially available, the instruments used, unless otherwise specified, can all be commercially available, and the processes involved, unless otherwise specified, are all routinely selected by those skilled in the art.

[0056] Example 1

[0057] This embodiment provides a photovoltaic module, the structure of which is shown in FIG. Figure 3, including a front cover plate 21, a plurality of battery cells 22, a film tape 23 and an organic light-transmitting back plate 24, wherein the plurality of battery cells 12 are arranged at intervals between the front cover plate 21 and the organic light-transmitting back plate 24, and the film tape 23 is located on a side of the organic light-transmitting back plate 24 close to the battery cells 22, wherein the front cover plate 21, the plurality of battery cells 22, the film tape 23 and the organic light-transmitting back plate 24 are bonded by a transparent adhesive film, and the film tape 23 includes a modified EVA layer 231, a PET support layer 232, a concave-convex structure 233, an insulating layer 234 and an aluminum reflective layer 235, wherein the PET support layer 232 is located on a side of the modified EVA layer 231 away from the organic light-transmitting back plate 14, the concave-convex structure 233 is located on a side of the PET support layer 232 away from the modified EVA layer 231, the insulating layer 234 is located on a side of the concave-convex structure 233 away from the PET support layer 232, and the aluminum reflective layer 235 is located on a side of the insulating layer 234 away from the concave-convex structure 233. The organic light-transmitting backplane 24 includes a modified coating 241, an organic matrix 242 and a protective coating 243. The organic matrix 242 is located on the side of the modified coating 241 away from the film strip 23, and the protective coating 243 is located on the side of the organic matrix 242 away from the modified coating 241. The modified coating 241 of the organic light-transmitting backplane 24 is in contact with the modified EVA layer 231 of the film strip 23. The crosslinking degree of the modified EVA layer is 70%, the VA content is 30wt%, and the thickness is 75μm. The position and size of the film strip correspond to the gap between two adjacent battery cells, and the width of the film strip is 2mm. The modified coating contains SiO2 particles, the surface roughness is 1.1μm, and the thickness is 80μm.

[0058] Comparative Example 1

[0059] This comparative example provides a photovoltaic module, the structure of which is shown in FIG. Figure 1 , including a front cover plate 11, a plurality of cells 12, a glaze layer 13 and an organic light-transmitting backplane 14, wherein the plurality of cells 12 are arranged at intervals between the front cover plate 11 and the organic light-transmitting backplane 14, the glaze layer 13 is located on the side of the organic light-transmitting backplane 14 close to the cells 12, and the front cover plate 11, the plurality of cells 12, the glaze layer 13 and the organic light-transmitting backplane 14 are bonded by a transparent adhesive film. The glaze layer 13 is formed by printing a glaze containing titanium dioxide (TiO2), and the glaze formula is: titanium dioxide, glass powder, organic binder, etc. The thickness of the glaze layer is 75μm. The position of the glaze corresponds to the gap between two adjacent cells, and the width is greater than the gap between two adjacent cells, and the glaze width is 6mm. The organic transparent backplane 14 comprises an organic matrix, a first protective coating on one side of the organic matrix, and a second protective coating on the other side of the organic matrix. The first protective coating is in contact with the glaze layer, and the coating is consistent with the coating without SiO2 particles added to the modified coating in Example 1, with a surface roughness of 0.55 μm and a thickness of 80 μm. The front cover 11, multiple battery cells 12, transparent adhesive film, organic matrix, and second protective coating are consistent with those in Example 1.

[0060] The photovoltaic modules of the above embodiments and comparative examples were tested according to the following method:

[0061] Project 1: Power test, refer to IEC61215 MQT06 test method, place the photovoltaic module under STC standard light (1000W / m 2 , 25℃ and IEC 60904-3 standard sunlight spectrum distribution), use the corresponding standard panel components as standard pieces to test the current, voltage and power of the photovoltaic components to be tested.

[0062] Project 2: Test of bifaciality: same as power test method, turn over the PV module to test the back side, bifaciality calculation formula = module back side power / module front side power * 100%.

[0063] Project 3: Test of aging resistance, refer to IEC61215 MQT13 damp heat test, test conditions: (85±2)℃, (85±5)% humidity, (1000+48)h, no pretreatment; during the test, the photovoltaic modules need to be short-circuited (except for samples of components that need to be powered on), open-circuited, (23±5)℃, less than 75% humidity, and recover for 2~4h;

[0064] The test results are shown in Table 1.

[0065] Table 1

[0066]

[0067] It can be seen that the power of the photovoltaic module of Example 1 is increased by 0.54% and the bifaciality is increased by 2.8% compared with Comparative Example 1. The photovoltaic module of Example 1 has excellent aging resistance and no delamination problem after the aging test.

[0068] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0069] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims.

Claims

1. A photovoltaic module, characterized in that: It includes a front cover, a plurality of battery cells, a film strip and an organic light-transmitting backplane, wherein the plurality of battery cells are arranged between the front cover and the organic light-transmitting backplane at intervals, and the film strip is located on a side of the organic light-transmitting backplane close to the battery cells; The film tape includes a modified EVA layer, the organic light-transmitting backplane includes a modified coating, the modified EVA layer is in contact with the modified coating, the crosslinking degree of the modified EVA layer is 65%~85%, the VA content is 28wt%~33wt%, and the surface roughness of the modified coating is 1.1μm±0.1μm.

2. The photovoltaic module according to claim 1, characterized in that: The raw materials of the modified EVA layer include a main resin and an auxiliary agent, wherein the main resin includes ethylene monomer and vinyl acetate monomer, and the auxiliary agent includes one or more of a coupling agent and a cross-linking agent.

3. The photovoltaic module according to claim 1, characterized in that: The film tape also includes a PET supporting layer, a concave-convex structure, an insulating layer and an aluminum reflecting layer; the PET supporting layer is located on the side of the modified EVA layer away from the organic light-transmitting backplane, the concave-convex structure is located on the side of the PET supporting layer away from the modified EVA layer, the insulating layer is located on the side of the concave-convex structure away from the PET supporting layer, and the aluminum reflecting layer is located on the side of the insulating layer away from the concave-convex structure.

4. The photovoltaic module according to claim 3, characterized in that: The film tape further comprises an EVA layer, wherein the EVA layer is located between the modified EVA layer and the PET support layer.

5. The photovoltaic module according to claim 1, characterized in that: Includes at least one of the following features: (1) The thickness of the modified EVA layer is 1 μm to 100 μm; (2) The thickness of the film tape is 50 μm to 150 μm.

6. The photovoltaic module according to claim 1, characterized in that: The position and size of the film strip corresponds to the gap between two adjacent battery cells, or a plurality of battery cells are connected in series to form a plurality of battery strings, and the position and size of the film strip corresponds to the gap between two adjacent battery strings.

7. The photovoltaic module according to any one of claims 1 to 6, characterized in that: The modified coating contains SiO2 particles.

8. The photovoltaic module according to claim 7, characterized in that: The SiO2 particles meet at least one of the following conditions: (1) The average particle size of the SiO2 particles is 5 μm ± 1 μm; (2) The mass proportion of the SiO2 particles in the modified coating is 5%±1%.

9. The photovoltaic module according to claim 8, characterized in that: The coating of the modified coating comprises a main resin, a functional additive and the SiO2 particles, the main resin comprises a fluorocarbon resin and an acrylic resin, and the functional additive comprises one or more of an ultraviolet absorber, a light stabilizer, an anti-hydrolysis agent, a leveling agent and a dispersant.

10. The photovoltaic module according to any one of claims 1 to 6, 8 to 9, characterized in that: The organic light-transmitting backplane further comprises an organic matrix and a protective coating, wherein the organic matrix is ​​located on a side of the modified coating away from the film strip, and the protective coating is located on a side of the organic matrix away from the modified coating.

Citation Information

Patent Citations

  • Photovoltaic module packaged by flexible component back plate and partitioned light-transmitting material and manufacturing method thereof

    CN102184991A

  • Transparent PET backboard of double-layered structure and processing method thereof

    CN109943040A

  • UV cut-off EPE photovoltaic adhesive film, preparation method thereof and photovoltaic module

    CN114806422A

  • Upconversion photovoltaic backboard and double-sided photovoltaic module

    CN115274901A

  • Composite bearing film for photovoltaic module, preparation method of composite bearing film and photovoltaic module

    CN116504859A

Cited By

  • Photovoltaic module and method for manufacturing photovoltaic module

    WO2026218549A1