High-nickel compound and positive pole piece containing same
By adopting high nickel compounds with low cobalt content and multiple coating processes, the high nickel compound positive electrode materials have been solved, and cost reduction and performance improvement have been achieved.
Patent Information
- Application Number
- CN202411082158.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-11-22
AI Technical Summary
The existing high-nickel compound positive electrode materials have a high cobalt content, which leads to an increase in raw material costs, and the preparation process has a great impact on the crystal structure and performance, affecting the structural stability and electrochemical properties of the material.
The chemical formula of high nickel compound with low cobalt content is LiaNixCoyMnzMbO2·cα·dβ. The residual alkali is reduced through multiple coating processes, and the solvent washing process is reduced. The doping element M and coatings α and β are used to improve structural stability and Lithium ion channel capacity.
It reduces raw material costs, improves the structural stability of the material and the capacity of lithium ion channel, enhances the rate performance and circulation performance of the positive electrode material, and reduces environmental protection issues in solvent recovery.
Smart Images

Figure CN119008884A_ABST
Abstract
Description
[0001] Divisional Application Information
[0002] This application is a divisional application of the invention patent application with application date of June 4, 2024, application number 202410715967.1, and invention name “High nickel compounds and preparation methods thereof”. Technical Field
[0003] The invention relates to the field of lithium ion batteries, and in particular to a high-nickel compound and a positive electrode sheet containing the same. Background Art
[0004] At present, with the rapid development of the new energy market, high-nickel lithium batteries (Ni molar fraction ≥ 0.6) as an environmentally friendly energy storage material have received more and more attention. The positive electrode material, as one of the most important components of lithium batteries, directly affects the performance of the battery, and the structural characteristics and preparation process of high-nickel compounds used for positive electrode materials play a decisive role in the performance and application of lithium batteries. For example, the high cobalt content of the raw materials used to prepare high-nickel compounds will increase the cost of raw materials, and the preparation process will also have a certain impact on the crystal structure and performance (such as electrochemical performance) of high-nickel compounds, thereby affecting the structural stability of the positive electrode material, rate performance, material storage, cycle performance and other aspects.
[0005] Therefore, the existing high-nickel compounds and positive electrode plates containing the same need to be further improved. Summary of the invention
[0006] One of the purposes of the present application is to provide a high-nickel compound and a positive electrode sheet containing the same, for example, a positive electrode sheet for forming a lithium battery.
[0007] An embodiment of the present application provides a high nickel compound, the general chemical formula of which is Li a Ni x Co y Mn z M b O2·cα·dβ, wherein 1≤a≤1.2, 0<b≤0.01, 0<c≤0.01, 0<d≤0.02, 0.8≤x≤1, 0≤y<0.12, 0≤z≤0.2, x+y+z=1; M is a doping element; α is a first coating, and β is a second coating.
[0008] Another embodiment of the present application further provides a positive electrode plate, which includes a positive electrode current collector and a positive electrode active material, and the positive electrode active material includes the above-mentioned high-nickel compound.
[0009] Yet another embodiment of the present application provides an electrode assembly, which includes: a negative electrode plate, which includes a negative electrode current collector and a negative electrode active material located on the negative electrode current collector; and the above-mentioned positive electrode plate.
[0010] The fourth embodiment of the present application further provides a battery, which includes the above-mentioned electrode assembly.
[0011] The fifth embodiment of the present application further provides an electrical device, which includes the above-mentioned battery, and the battery is used to provide electrical energy.
[0012] The sixth embodiment of the present application also provides a method for preparing a high-nickel compound, which comprises:
[0013] (1) mixing a lithium source, a nickel-cobalt-manganese precursor and an M source, and performing a first calcination treatment to prepare a first main material, wherein the M source is a compound containing an element M, and the general formula of the first main material is Li a Ni x Co y Mn z M b O2, 1≤a≤1.2, 0<b≤0.01, 0.8≤x≤1, 0≤y<0.12, 0≤z≤0.2, x+y+z=1;
[0014] (2) mixing the first main material with the A source and performing a second roasting treatment to prepare a second main material, wherein the A source is a compound containing the element A;
[0015] (3) The second main material is mixed with a B source and subjected to a third roasting treatment, wherein the B source is a compound containing elemental boron.
[0016] Compared with the prior art, the high-nickel compound and the positive electrode plate containing the same provided in the embodiments of the present application have a low cobalt content, which can reduce costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The following will briefly describe the drawings necessary for describing the embodiments of the present application or the prior art to facilitate the description of the embodiments of the present application. Obviously, the drawings described below are only some of the embodiments in the present application. For those skilled in the art, without the need for creative work, drawings of other embodiments can still be obtained based on the structures illustrated in these drawings.
[0018] Figure 1 Schematic diagram of a method for preparing high-nickel compounds according to some embodiments of the present application. DETAILED DESCRIPTION
[0019] In order to better understand the spirit of the embodiments of the present application, some preferred embodiments of the present application are further described below.
[0020] Embodiments of the present application will be described in detail below. Throughout the present application specification, as used herein, the term "about" is used to describe and illustrate small changes. When used in conjunction with an event or situation, the term may refer to an example in which an event or situation occurs precisely and an example in which an event or situation occurs very approximately. For example, when used in conjunction with a numerical value, the term may refer to a range of variation of less than or equal to ±10% of the numerical value, such as less than or equal to ±5%, less than or equal to ±4%, less than or equal to ±3%, less than or equal to ±2%, less than or equal to ±1%, less than or equal to ±0.5%, less than or equal to ±0.1%, or less than or equal to ±0.05%. For example, two values may be considered to be “approximately” the same if the difference between them is less than or equal to ±10% of the mean of the values (e.g., less than or equal to ±5%, less than or equal to ±4%, less than or equal to ±3%, less than or equal to ±2%, less than or equal to ±1%, less than or equal to ±0.5%, less than or equal to ±0.1%, or less than or equal to ±0.05%).
[0021] In this specification, amounts, ratios and other numerical values are sometimes presented herein in a range format. It should be understood that such a range format is used for convenience and brevity, and should be flexibly understood to include not only the values explicitly specified as range limits, but also all individual values or sub-ranges encompassed within the range, as if each value and sub-range were explicitly specified.
[0022] In addition, for convenience of description, the words "first", "second", etc. may be used herein to distinguish one substance or a series of substances, and these words may be construed as names.
[0023] The general chemical formula of the high nickel compound proposed in this application is Li a Ni x Co y Mn z M b O2·cα·dβ, wherein: 1.00≤a≤1.20, 0.00<b≤0.01, 0.00<c≤0.01, 0.00<d≤0.02, 0.80≤x<1.00, 0.00≤y<0.12, 0.00≤z<0.2, x+y+z=1; M is a doping element; α is a first coating, and β is a second coating.
[0024] The high-nickel compound proposed in the present application greatly reduces the raw material cost because the raw materials used have a relatively low cobalt content.
[0025] For high-nickel positive electrode materials with a nickel mole fraction exceeding about 0.6, for example, high-nickel positive electrode materials with a nickel mole fraction exceeding about 0.8, multiple coating processes can appropriately reduce residual alkali and reduce or even avoid the use of solvent washing recovery processes.
[0026] The doping element M is used to partially replace the spatial position of nickel, cobalt and manganese. During the charge and discharge process, it stabilizes the skeleton structure, inhibits structural collapse, and stabilizes the spatial structure. At the same time, due to the relatively large ion radius, it can provide a larger lithium ion channel and improve the material capacity. For example, the element M can be selected from one or more elements of the VB and VIB groups.
[0027] The first coating material α is used for shallow coating and is enriched on the surface of the primary particles. During the charge and discharge process, it can effectively release the stress generated by the primary particles during the volume change process and improve the stability of the primary particles. For example, α can be selected from a compound containing one or more elements of the VB and VIB group elements. For example, α is WO3, MoO3, or Nb2O5.
[0028] The second coating β is used for surface coating to prevent the positive electrode material from directly contacting the electrolyte, inhibit the side reaction between the positive electrode material and the electrolyte, and improve the safety performance. For example, β can be selected from one or more of boric acid, lithium borate, lithium metaborate, lithium tetraborate and other boron-containing compounds, or a compound formed by one or more of boric acid, lithium borate, lithium metaborate, lithium tetraborate and other boron-containing compounds. Exemplarily, β can be Li3BO3, LiBO2, Li2B4O7.
[0029] According to some embodiments of the present application, the specific surface area of the high nickel compound may be about 0.1-1.5 m 2 / g, and an average particle size of about 2-15 μm. For example, the average particle size of the high-nickel compound is about 5-15 μm, and it can be a single crystal or a polycrystalline compound. By mass, the high-nickel compound contains less than about 1500 ppm of total free lithium.
[0030] According to some embodiments of the present application, in the X-ray diffraction spectrum of the above-mentioned high-nickel compound, the ratio of the half-maximum width FWHM(006) of the (006) diffraction peak near about 37.9° to the half-maximum width FWHM(102) of the (102) diffraction peak near about 38.2° is about 1.05 to 1.15.
[0031] According to some embodiments of the present application, in the X-ray diffraction spectrum of the above-mentioned high-nickel compound, the ratio of the half-maximum width FWHM(108) of the (108) diffraction peak near about 64.3° to the half-maximum width FWHM(110) of the (110) diffraction peak near about 64.7° is about 0.95 to 1.05.
[0032] According to some embodiments of the present application, the high-nickel compound can be used as a positive electrode material for lithium-ion batteries. For example, the high-nickel compound, conductive carbon black (SP), and adhesive polyvinylidene fluoride (PVDF) are added to N-methylpyrrolidone (NMP) (the weight ratio of the high-nickel compound to NMP is 2.1:1) at a weight ratio of 94:3:3, and the mixture is fully mixed, stirred to form a uniform slurry to prepare a positive electrode material (or positive electrode active material), coated on an aluminum foil current collector, dried, and pressed to obtain a positive electrode sheet, which can constitute an electrode assembly with a negative electrode sheet.
[0033] The present application also provides a battery, which may be a lithium-ion battery, comprising the above-mentioned electrode assembly. The lithium-ion battery may be used in digital products, electric vehicles or energy storage fields.
[0034] For example, a lithium-ion secondary battery can generally be composed of an electrode assembly, a non-aqueous electrolyte, a separator and a container. Specifically, the electrode assembly may include a positive electrode sheet and a negative electrode sheet. As mentioned above, the positive electrode sheet may be made of materials including a positive electrode current collector and a positive electrode active material coated on the positive electrode current collector, as well as conventional adhesives, conventional conductive additives and the like. The positive electrode active material may include the above-mentioned high-nickel compound proposed in this application. The negative electrode is made of materials including a current collector and a conventional negative electrode active material coated on the current collector, as well as conventional adhesives, conventional conductive additives and the like. The separator is a PP / PE film commonly used in this industry, which is used to separate the positive electrode from the negative electrode. The container is a container for the positive electrode, the negative electrode, the separator and the electrolyte.
[0035] When a 1 mol / L lithium hexafluorophosphate solution is used as the electrolyte, the solvent in the lithium hexafluorophosphate solution is a mixed solvent of dimethyl carbonate (DMC): ethylene carbonate (EC): diethyl carbonate (DEC) = 1:1:1, a mixture of artificial graphite, conductive carbon black, carboxymethyl cellulose and adhesive in a weight ratio of 95:1:1:3 is used as the negative electrode material, and a mixture of the above-mentioned high nickel compound, conductive carbon black and PVDF in a weight ratio of 94:3:3 is used to prepare the positive electrode sheet, and then a battery cell is prepared, the model is 454261, and finally a battery is formed.
[0036] Some embodiments of the present application further provide an electrical device, which includes the above-mentioned battery, and the above-mentioned battery is used to provide power. The electrical device may include digital products, electric vehicles, energy storage devices, etc. For example, it can be used in portable electronic devices and electric vehicles, and can also be used in energy storage power supply systems such as hydropower, thermal power, wind power and solar power stations.
[0037] As people pay more and more attention to environmental protection, new energy is becoming more and more popular. Lithium-ion batteries, as one of the power batteries used in new energy vehicles, have broad application prospects.
[0038] Some other embodiments of the present application also provide a method for preparing the above-mentioned high-nickel compound, which comprises the following steps:
[0039] (1) mixing a lithium source, a nickel-cobalt-manganese precursor and an M source, and performing a first calcination treatment to prepare a first main material, wherein the M source is a compound containing an element M, and the general formula of the first main material is Li a Ni x Co y Mn z M b O2, 1≤a≤1.2, 0<b≤0.01, 0.8≤x≤1, 0≤y<0.12, 0≤z≤0.2, x+y+z=1;
[0040] (2) mixing the first main material with the A source and performing a second roasting treatment to prepare a second main material, wherein the A source is a compound containing the element A;
[0041] (3) The second main material is mixed with a B source and subjected to a third roasting treatment, wherein the B source is a compound containing elemental boron.
[0042] The general chemical formula of the second main material can be Li a Ni x Co y Mn z M b O2·cα, wherein α is the first coating.
[0043] Generally, the residual alkali in high-nickel compounds can be reduced by solvent washing, but this method involves solvent recovery and environmental protection issues. The present application proposes to use multiple coating processes to minimize or even avoid solvent recovery issues.
[0044] According to some embodiments of the present application, the lithium source may be selected from lithium hydroxide monohydrate. The M source is a compound containing element M, and the element M may be selected from one or more of VB and VIB group elements. Exemplarily, the M source may be tantalum oxide, niobium oxide, molybdenum oxide, or tungsten oxide.
[0045] According to some embodiments of the present application, the nickel-cobalt-manganese precursor is one or more of hydroxides, carboxyl oxides or oxides containing nickel, cobalt and manganese elements, and the particle size may be about 3 μm-15 μm.
[0046] According to some embodiments of the present application, the element A may be selected from one or more of the elements of the VB and VIB groups. For example, the source of A may be selected from one or more of tungsten oxide, molybdenum oxide, and niobium oxide.
[0047] According to some embodiments of the present application, the B source may be selected from one or more of boric acid, lithium borate, lithium metaborate and lithium tetraborate.
[0048] According to some embodiments of the present application, the mass ratio of the first main material to the source A is about 1.0:(0.002-0.01), for example, about 1:(0.003-0.007). The mass ratio of the second main material to the source B is 1:
[0049] (0.002~0.01), for example, is about 1:(0.002~0.005).
[0050] According to some embodiments of the present application, in the above preparation method, the first roasting temperature is about 700-900°C, for example, about 700-850°C, and the first roasting time is about 8-30 hours, for example, about 20-24 hours; the second roasting temperature is about 500-800°C, for example, about 700-800°C, and the second roasting time is about 6-20 hours, for example, about 12-18 hours; the third roasting temperature is about 250-450°C, for example, about 300-400°C, and the third roasting time is about 3-15 hours, for example, about 6-10 hours.
[0051] According to some embodiments of the present application, in the above preparation method, the first calcination temperature is about 780°C, 800°C, or 840°C, and the first calcination time is about 20 hours or about 24 hours; the second calcination temperature is about 700°C, 740°C, or 780°C, and the second calcination time is about 10 hours, 12 hours, 16 hours, or 18 hours; the third calcination temperature is about 280°C, 350°C, 400°C, or 450°C, and the third calcination time is about 6 hours or 8 hours.
[0052] The method for preparing high-nickel compounds proposed in this application is convenient for large-scale production. The residual alkali in the high-nickel compound can be significantly reduced by high-temperature roasting, and a solvent-free process can be used to reduce or avoid environmental problems of solvent recovery. Combined with the second coating process, the capacity of the positive electrode material will be further improved. The temperature of the first roasting treatment is relatively high, which can stabilize the structure and interface; the temperature of the second and third roasting treatments is relatively low, which can inhibit the side reactions of the positive electrode material and the electrolyte. By reducing the loss of lithium metal, the capacity of the high-nickel compound can be significantly improved.
[0053] Usually, the positive electrode materials formed by high-nickel compounds have high residual alkali, so most of them are washed with solvents to wash away the excess residual alkali. However, solvent washing will lead to waste of lithium ions, and more lithium salts need to be added to the ingredients. The preparation method of high-nickel compounds proposed in this application increases the number of roasting treatments, which can effectively reduce residual alkali and modify interface defects, thereby reducing or even avoiding solvent washing in process design, and relatively small amounts of lithium salts can be added to the ingredients. This process, coupled with a specific crystal half-width ratio, can maximize the role of lithium ions, and the synthesized positive electrode material has a higher capacity and better gas production performance.
[0054] The high-nickel compound and its preparation method and application proposed in the present application are described below by specific examples. The reagents or instruments not described in the present application are all contents that can be routinely confirmed by ordinary technicians in the field.
[0055] The reagents used in the following examples are shown in Table 1-1.
[0056] Table 1-1 Reagent information used in the examples of this application
[0057]
[0058]
[0059] The equipment and analysis methods used in the following examples are as follows:
[0060] The pulverizing equipment is the SHQM double planetary mill produced by Lianyungang Chunlong Experimental Instrument Co., Ltd.; the air flow pulverizing equipment is the MX-50 air flow pulverizer produced by Yixing Juneng Pulverizing Equipment Co., Ltd.
[0061] This application uses a fully automatic specific surface area and porosity analyzer (TriStarⅡ3020, Murray McTick Co., Ltd., USA) to test and analyze the specific surface area.
[0062] The test method for free lithium in high nickel compounds is as follows:
[0063] Accurately weigh an appropriate amount of sample m grams (about 30g), accurate to 0.01g; put the sample into a 250mL conical flask, put in a magnetic stirring bar, and add 100mL deionized water; put the conical flask on a magnetic stirrer, turn on the stirrer and stir for 30 minutes; filter the mixed solution with filter paper and funnel; use a 50mL pipette to transfer 50mL of filtrate, put it into a 100mL beaker, and put in a magnetic stirring bar; put the beaker on a magnetic stirrer and add 2 drops of phenolphthalein indicator; titrate with 0.05mol / L hydrochloric acid standard titration solution until the color of the solution changes from red to colorless; record the volume V1 (end point 1) of the 0.05mol / L hydrochloric acid standard titration solution; add 2 drops of methyl red indicator and the color changes from colorless to yellow; titrate with 0.05mol / L hydrochloric acid standard titration solution Titrate until the color of the solution changes from yellow to orange; place the beaker on a heating furnace and heat until the solution boils (the color of the solution changes from orange to yellow); remove the 100mL beaker and cool to room temperature; place the beaker on a magnetic stirrer again; titrate with 0.05mol / L hydrochloric acid standard titration solution until the color of the solution changes from yellow to light red; record the volume V2 of the 0.05mol / L hydrochloric acid standard titration solution (end point 2); lithium hydroxide: LiOH (wt%) = [V2-2×(V2-V1)]×0.05×23.946×2×100 / (m×1000); lithium carbonate: Li2CO3 (wt%) = (V2-V1)×0.05×73.886×2×100 / (m×1000); free lithium: Li + (wt%)=V2×0.05×6.94×2×100 / (m×1000).
[0064] Average particle size test: MS3000 laser particle size analyzer is used for testing, the method is as follows:
[0065] Take an appropriate amount of sample in a 100ml beaker, first rinse along the inner wall of the beaker with a wash bottle, then rinse the sample stuck to the bottom of the beaker with a wash bottle, and control the amount of pure water added to the beaker to 20-30mL, and the ultrasonic time is 5min (stir for 10s before, during and after ultrasonication, and the stirring rate is about 2r / s). Add 100±10ml of pure water to the injector of the MS3000 laser particle size analyzer, adjust the speed to 3000r / min, click start, and the instrument will automatically align the light and measure the background and wait for prompts to operate. Transfer the sample after ultrasonication to the stirring tank, and then rinse the beaker with a wash bottle to ensure that all samples are transferred. After the sample is completely added, the software automatically starts measuring. After the measurement is completed, the data is automatically saved.
[0066] X-ray diffraction test method: The test was carried out using the Netherlands Paneck pert PRU X-ray diffractometer, with Cu- as the ray source and a diffraction angle of 10-80°.
[0067] The method for preparing a battery (cell model 454261) using the high nickel compound prepared in this application is as follows:
[0068] Preparation of positive electrode sheet: The high nickel compound proposed in this application is added to N-methylpyrrolidone (NMP) (the weight ratio of the high nickel compound to NMP is 2.1:1) in a weight ratio of 94:3:3, and the mixture is stirred to form a uniform slurry, which is then coated on an aluminum foil current collector, dried and pressed into a electrode sheet.
[0069] Preparation of negative electrode sheets: Add negative electrode artificial graphite, conductive carbon black (SP), carboxymethyl cellulose (CMC), and adhesive (SBR) in a weight ratio of 95:1:1:3 into sufficient pure water, stir to form a uniform slurry, apply it on the copper foil current collector, dry and press into a sheet.
[0070] The diaphragm is a three-layer composite film material of PP / PE / PP.
[0071] The pressed positive and negative electrode sheets are spot welded to the upper pole ears, and after inserting the diaphragm, they are wound on the winder and loaded into the soft package fixture, and the top and side are sealed. Then, they are placed in an oven for baking, and then 9g of electrolyte is injected in an environment with a relative humidity of less than 1.5%. After the electrolyte is injected and formed for 48 hours (Zhejiang Hangke LIP-3AHB06 high constant temperature formation system), vacuum sealing is performed.
[0072] The sample drying and battery high temperature testing were carried out using the Dongguan Kerui Electromechanical KPBAK-03E-02 high-efficiency vacuum drying oven.
[0073] The charge and discharge test of the lithium-ion secondary battery prepared in this application is tested on the Wuhan Blue Electric Battery Tester (Wuhan Blue Electric CT2001C test equipment) according to the test method of GB / T18287-2000. Due to different battery systems, the cycle retention rate of the material is greatly affected. The battery system used in the experiment is the most common evaluation system, that is, a 1mol / L lithium hexafluorophosphate solution is used as the electrolyte, and the solvent in the lithium hexafluorophosphate solution is a mixed solvent with a mass ratio of dimethyl carbonate (DMC): ethylene carbonate (EC): diethyl carbonate (DEC) = 1:1:1, and a mixture of artificial graphite and conductive carbon black, carboxymethyl cellulose and adhesive in a weight ratio of 95:1:1:3 is used as the negative electrode material, and the battery model is 454261, so as to expose the actual defects of the positive electrode material as soon as possible and determine the performance of the positive electrode material.
[0074] Example 1
[0075] According to the molar ratio of Li: (Ni + Co + Mn): Nb = 1.03: 1: 0.004, lithium hydroxide monohydrate and a precursor (chemical formula: Ni) with a molar ratio of Ni: Co: Mn = 92: 05: 03 were added. 0.92 Co 0.05 Mn 0.03 (OH)2) and nano niobium pentoxide powder are ball milled at a speed of 40HZ for 10 minutes to mix evenly and then discharged (i.e., mixed material). The mixed material is placed in a muffle furnace, heated to 780°C at a heating rate of 5°C / min in an oxygen atmosphere, sintered for 24 hours, cooled to room temperature, and ball milled at a speed of 40HZ for 10 minutes to obtain the first main material; then, according to the mass ratio of the first main material: tungsten oxide of 1.0:0.0028, a corresponding amount of tungsten oxide is weighed and added to the first main material for ball milling, ball milled at a speed of 40HZ for 10 minutes, the mixed material is placed in a muffle furnace, heated to 700°C at a heating rate of 10°C / min in an oxygen atmosphere, sintered for 18 hours (second sintering), and cooled to room temperature. The sample after the second sintering is crushed to obtain the second main material. Then, according to the mass ratio of the second main material to boric acid of 1.0:0.0025, a corresponding amount of boric acid was weighed and added to the second main material for ball milling, and the ball milling was carried out at a rotation speed of 40HZ for 10 minutes. The evenly mixed materials were placed in a muffle furnace, and the temperature was increased to 350°C at a heating rate of 5°C / min in an air atmosphere and sintered for 6 hours. The mixture was cooled to room temperature and sieved with a 300-mesh metal screen to obtain a high-nickel compound 1.
[0076] The particle size of high nickel compound 1 was tested, and the average particle size of primary particles was 10.5 μm.
[0077] The high nickel compound 1 was subjected to comparative table, X-ray diffraction and cycle test, and the data are shown in Table 8.
[0078] The element composition of high nickel compound 1 was analyzed, and the test data are shown in Table 1. The chemical formula of the high nickel compound finally obtained is Li 1.03 Ni 0.92 Co 0.05 Mn 0.03 Nb 0.004 O2·0.0012WO30.004 Li3BO3.
[0079] The test method for element content is as follows:
[0080] Accurately weigh 0.2000g (accurate to 0.0001g) of the sample into a clean 100mL glass beaker. Add 10mL (1:1) aqua regia solution to the beaker (conduct a blank experiment together), cover with a watch glass, place the beaker on a hot plate and heat the solution until it evaporates to near dryness, then stop heating, remove the beaker and cool to room temperature. Rinse the watch glass and the side of the beaker with deionized water at least 3 times, transfer all the solution to a 50mL volumetric flask, dilute to volume with deionized water, and shake well. Transfer 1mL of the sample to a 100mL volumetric flask, dilute to volume, and shake well. Test the above solution using an inductively coupled plasma emission spectrometer (Thermo Fisher Scientific Inc. / icap7400, USA) in accordance with the first part of YS / T 1006.2-2014.
[0081] Table 1 Test results of element mass content of high nickel compounds 1
[0082] element Li Ni Co Mn Nb W B % 7.2532 54.8892 2.9952 1.6753 0.3777 0.2242 0.0439
[0083] Example 2
[0084] According to the molar ratio of Li: (Ni + Co + Mn): Ta = 1.10: 1: 0.003, lithium hydroxide monohydrate and a precursor with a molar ratio of Ni: Co: Mn = 93: 03: 04 (chemical formula: Ni 0.93 Co 0.03 Mn 0.04 (OH)2) and nano tantalum oxide powder are ball milled at a speed of 40HZ for 10 minutes to mix evenly and then discharged (i.e., mixed material). The mixed material is placed in a muffle furnace, heated to 800℃ at a heating rate of 5℃ / min in an oxygen atmosphere, sintered for 20 hours, cooled to room temperature, ball milled at a speed of 40HZ for 10 minutes, and then air flow crushed to obtain the first main material. Then, according to the mass ratio of the first main material: molybdenum oxide of 1.0:0.003, the corresponding amount of molybdenum oxide is weighed and added to the first main material for ball milling, ball milled at a speed of 40HZ for 10 minutes, the mixed material is placed in a muffle furnace, heated to 700℃ at a heating rate of 10℃ / min in an oxygen atmosphere, sintered for 12 hours (second sintering), and cooled to room temperature. The sample after the second sintering is crushed to obtain the second main material. Then, according to the mass ratio of the second main ingredient: lithium borate of 1.0:0.005, a corresponding amount of lithium borate was weighed and added to the main ingredient 2 for ball milling, and the ball milling was carried out at a rotation speed of 40HZ for 10 minutes. The evenly mixed materials were placed in a muffle furnace, and the temperature was increased to 450°C at a heating rate of 5°C / min in an air atmosphere and sintered for 8 hours. The mixture was cooled to room temperature and sieved with a 300-mesh metal screen to obtain a high-nickel compound 2.
[0085] The particle size of high nickel compound 2 was tested, and the average particle size of primary particles was 3.8 μm.
[0086] The high nickel compound 2 was subjected to comparative table, X-ray diffraction and cycle test, and the data are shown in Table 8.
[0087] The element composition of high nickel compound 2 was analyzed, and the test data are shown in Table 2. The chemical formula of the high nickel compound finally obtained is Li 1.10 Ni 0.93 Co 0.03 Mn 0.04 Ta 0.003 O2·0.002MoO30.008 Li3BO3.
[0088] The test method for element content is as follows:
[0089] Accurately weigh 0.2000g (accurate to 0.0001g) of the sample into a clean 100mL glass beaker. Add 10mL (1:1) aqua regia solution to the beaker (conduct a blank experiment together), cover with a watch glass, place the beaker on a hot plate and heat the solution until it evaporates to near dryness, then stop heating, remove the beaker and cool to room temperature. Rinse the watch glass and the side of the beaker with deionized water at least 3 times, transfer all the solution to a 50mL volumetric flask, dilute to volume with deionized water, and shake well. Transfer 1mL of the sample to a 100mL volumetric flask, dilute to volume, and shake well. Test the above solution using an inductively coupled plasma emission spectrometer (Thermo Fisher Scientific Inc. / icap7400, USA) in accordance with the first part of YS / T 1006.2-2014.
[0090] Table 2 Test results of mass content of 2 elements in high nickel compounds
[0091] element Li Ni Co Mn Ta Mo B % 7.6944 55.1332 1.7857 2.2195 0.5481 0.1938 0.0873
[0092] Example 3
[0093] According to the molar ratio of Li: (Ni + Co + Mn): W = 1.2: 1: 0.002, lithium hydroxide monohydrate and a precursor with a molar ratio of Ni: Co: Mn = 83: 07: 10 (chemical formula: Ni 0.83 Co 0.07 Mn 0.10(OH)2) and nano tungsten oxide powder are ball milled at a speed of 40HZ for 10 minutes to mix evenly and then discharged (i.e., mixed material). The mixed material is placed in a muffle furnace, heated to 840℃ at a heating rate of 5℃ / min in an oxygen atmosphere and sintered for 24 hours, cooled to room temperature, ball milled at a speed of 40HZ for 10 minutes and then air flow crushed to obtain the first main material. Then, according to the mass ratio of the first main material: niobium oxide of 1.0:0.0067, the corresponding amount of niobium oxide is weighed and added to the first main material for ball milling, ball milled at a speed of 40HZ for 10 minutes, the mixed material is placed in a muffle furnace, heated to 780℃ at a heating rate of 10℃ / min in an oxygen atmosphere and sintered for 18 hours (second sintering), and cooled to room temperature. The sample after the second sintering is crushed to obtain the second main material. Then, according to the mass ratio of the second main ingredient: lithium metaborate of 1.0:0.004, a corresponding amount of lithium metaborate was weighed and added to the main ingredient 2 for ball milling, and the ball milling was carried out at a rotation speed of 40HZ for 10 minutes. The evenly mixed materials were placed in a muffle furnace, and the temperature was increased to 400°C at a heating rate of 5°C / min in an air atmosphere and sintered for 8 hours. The mixture was cooled to room temperature and sieved with a 300-mesh metal screen to obtain a high-nickel compound 3.
[0094] The particle size of high nickel compound 3 was tested, and the average particle size of primary particles was 4.2 μm.
[0095] The high nickel compound 3 was subjected to comparative table, X-ray diffraction and cycle test, and the data are shown in Table 8.
[0096] The element composition of high nickel compound 3 was analyzed, and the test data are shown in Table 3. The chemical formula of the high nickel compound finally obtained is Li 1.2 Ni 0.83 Co 0.07 Mn 0.10 W 0.002 O2·0.0025Nb2O50.008 LiBO2.
[0097] The test method for element content is as follows:
[0098] Accurately weigh 0.2000g (accurate to 0.0001g) of the sample into a clean 100mL glass beaker. Add 10mL (1:1) aqua regia solution to the beaker (conduct a blank experiment together), cover with a watch glass, place the beaker on a hot plate and heat the solution until it evaporates to near dryness, then stop heating, remove the beaker and cool to room temperature. Rinse the watch glass and the side of the beaker with deionized water at least 3 times, transfer all the solution to a 50mL volumetric flask, dilute to volume with deionized water, and shake well. Transfer 1mL of the sample to a 100mL volumetric flask, dilute to volume, and shake well. Test the above solution using an inductively coupled plasma emission spectrometer (Thermo Fisher Scientific Inc. / icap7400, USA) in accordance with the first part of YS / T 1006.2-2014.
[0099] Table 3 Test results of mass content of three elements in high nickel compounds
[0100] element Li Ni Co Mn W Nb B % 8.2578 48.9203 4.1426 5.5169 0.3691 0.4665 0.0868
[0101] Example 4
[0102] According to the molar ratio of Li: (Ni + Co + Mn): Mo = 1.06: 1: 0.003, lithium hydroxide monohydrate and a precursor with a molar ratio of Ni: Co: Mn = 83: 07: 10 (chemical formula: Ni 0.83 Co 0.07 Mn 0.1 (OH)2) and nano molybdenum oxide powder are ball milled at a speed of 40HZ for 10 minutes to mix evenly and then discharged (i.e., mixed material). The mixed material is placed in a muffle furnace, heated to 800℃ at a heating rate of 5℃ / min in an oxygen atmosphere, sintered for 24 hours, cooled to room temperature, and ball milled at a speed of 40HZ for 10 minutes to obtain the first main material. Then, according to the mass ratio of the first main material: tungsten oxide of 1.0:0.0047, the corresponding amount of tungsten oxide is weighed and added to the first main material for ball milling, and the ball milling is carried out at a speed of 40HZ for 10 minutes. The uniformly mixed material is placed in a muffle furnace, heated to 740℃ at a heating rate of 10℃ / min in an oxygen atmosphere, sintered for 18 hours (second sintering), and cooled to room temperature. The sample after the second sintering is crushed to obtain the second main material. Then, according to the mass ratio of the second main material to lithium tetraborate of 1.0:0.0043, a corresponding amount of lithium tetraborate was weighed and added to the second main material for ball milling, and the ball milling was carried out at a rotation speed of 40HZ for 10 minutes. The evenly mixed materials were placed in a muffle furnace, and the temperature was increased to 280°C at a heating rate of 5°C / min in an air atmosphere and sintered for 8 hours. The mixture was cooled to room temperature and sieved with a 300-mesh metal screen to obtain a high-nickel compound 4.
[0103] The particle size of high nickel compound 4 was tested, and the average particle size of primary particles was 10.5 μm.
[0104] The high nickel compound 4 was subjected to comparative table, X-ray diffraction and cycle test, and the data are shown in Table 8.
[0105] The element composition of high nickel compound 4 was analyzed, and the test data are shown in Table 4. The chemical formula of the high nickel compound finally obtained is Li 1.08 Ni 0.83 Co 0.07 Mn 0.10 Mo 0.003 O2·0.002WO30.0025Li2B4O7.
[0106] Table 4 Test results of mass content of 4 elements in high nickel compounds
[0107] element Li Ni Co Mn Mo W B % 7.4456 49.4106 4.1841 5.5721 0.2919 0.3728 0.1094
[0108] Example 5
[0109] According to the molar ratio of Li: (Ni + Co + Mn): Nb = 1.1: 1: 0.001, lithium hydroxide monohydrate and a precursor with a molar ratio of Ni: Co: Mn = 87: 05: 08 (chemical formula: Ni 0.87 Co 0.05 Mn 0.08 (OH)2) and nano niobium oxide powder are ball milled at a speed of 40HZ for 10 minutes to mix evenly and then discharged (i.e., mixed material). The mixed material is placed in a muffle furnace, heated to 780°C at a heating rate of 5°C / min in an oxygen atmosphere and sintered for 20 hours, cooled to room temperature, and ball milled at a speed of 40HZ for 10 minutes to obtain the first main material. Then, according to the mass ratio of the first main material: tungsten oxide of 1.0:0.0047, the corresponding amount of tungsten oxide is weighed and added to the first main material for ball milling, and the ball milling is carried out at a speed of 40HZ for 10 minutes. The uniformly mixed material is placed in a muffle furnace, heated to 700°C at a heating rate of 10°C / min in an oxygen atmosphere, sintered for 16 hours (second sintering), and cooled to room temperature. The sample after the second sintering is crushed to obtain the main material 2 for the positive electrode material. Then, according to the mass ratio of main material 2: boric acid of 1.0:0.0048, a corresponding amount of boric acid was weighed and added to main material 2 for ball milling. The ball milling was carried out at a rotation speed of 40HZ for 10 min. The evenly mixed materials were put into a muffle furnace, and the temperature was increased to 350°C at a heating rate of 5°C / min in an air atmosphere and sintered for 6 hours. The mixture was cooled to room temperature and sieved with a 300-mesh metal screen to obtain high-nickel compound 5.
[0110] The particle size of high nickel compound 5 was tested, and the average particle size of primary particles was 11.2 μm.
[0111] The high nickel compound 5 was subjected to comparative table, X-ray diffraction and cycle test, and the data are shown in Table 8.
[0112] The element composition of high nickel compound 5 was analyzed, and the test data are shown in Table 5. The chemical formula of the final compound is Li 1.1 Ni 0.87 Co 0.05 Mn 0.08 Nb 0.001 O2·0.002WO30.006 Li3BO3.
[0113] Table 5 Test results of mass content of 5 elements in high nickel compounds
[0114] element Li Ni Co Mn Nb W B % 7.6837 51.8073 2.9895 4.4591 0.0942 0.3729 0.0658
[0115] Comparative Example 1
[0116] According to the molar ratio of Li: (Ni + Co + Mn): Nb = 1.12: 1: 0.002, lithium hydroxide monohydrate and a precursor with a molar ratio of Ni: Co: Mn = 83: 07: 10 (chemical formula: Ni 0.83 Co 0.07 Mn 0.1 (OH)2) and nano niobium oxide powder are ball milled at a speed of 40HZ for 10 minutes to mix evenly and then discharged (i.e., mixed material). The mixed material is placed in a muffle furnace and sintered at a temperature of 860°C at a heating rate of 5°C / min for 24 hours under an oxygen atmosphere, cooled to room temperature, ball milled at a speed of 40HZ for 10 minutes, and then air flow crushed to obtain the first main material. Then, the mass ratio of water: first main material: tungsten oxide is 1.5:
[0117] 1.0:0.007, add water and main material in turn, mix and stir for 10 minutes, then add tungsten oxide, continue stirring for 10 minutes, filter, and dry at 120℃. The dried sample is heated to 780℃ in an oxygen atmosphere at a heating rate of 10℃ / min and sintered for 10 hours (second sintering), and cooled to room temperature. The sample after the second sintering is crushed and sieved with a 300-mesh metal screen to obtain high-nickel compound D1.
[0118] The particle size of the high nickel compound D1 was tested, and the average particle size of the primary particles was 3.4 μm.
[0119] The high nickel compound D1 was subjected to comparative table, X-ray diffraction and cycle test, and the data are shown in Table 8.
[0120] The element composition of the high nickel compound D1 was analyzed, and the test data are shown in Table 6. The chemical formula of the final positive electrode material is Li 1.12 Ni 0.83 Co 0.07 Mn 0.10 Nb 0.002 O2·0.003WO3.
[0121] Table 6 The test results of element mass content of high nickel compound D1 are as follows
[0122] element Li Ni Co Mn Nb W % 7.7428 49.2849 4.1735 5.5582 0.1879 0.5578
[0123] Comparative Example 2
[0124] According to the molar ratio of Li: (Ni + Co + Mn): W = 1.06: 1: 0.001, lithium hydroxide monohydrate and a precursor with a molar ratio of Ni: Co: Mn = 83: 07: 10 (chemical formula: Ni 0.83 Co 0.07 Mn 0.1 (OH)2) and nano tungsten oxide powder are ball milled at a speed of 40HZ for 10 minutes to mix evenly and then discharged (i.e., mixed material), the mixed material is placed in a muffle furnace, heated to 780°C at a heating rate of 5°C / min in an oxygen atmosphere, sintered for 24 hours, cooled to room temperature, and ball milled at a speed of 40HZ for 10 minutes to obtain the first main material. Then, according to the mass ratio of the first main material: boric acid of 1.0:0.0043, the corresponding amount of boric acid is weighed and added to the main material 1 for ball milling, ball milled at a speed of 40HZ for 10 minutes, the mixed material is placed in a muffle furnace, heated to 320°C at a heating rate of 5°C / min in an air atmosphere, sintered for 8 hours, cooled to room temperature, and sieved with a 300-mesh metal screen to obtain a high-nickel compound D2.
[0125] The particle size of the high nickel compound D2 was tested, and the average particle size of the primary particles was 9.6 μm.
[0126] The high nickel compound D2 was subjected to comparative table, X-ray diffraction and cycle test, and the data are shown in Table 8.
[0127] The element composition of the high nickel compound D2 was analyzed, and the test data are shown in Table 7. The chemical formula of the final positive electrode material is Li 1.06 Ni 0.83 Co 0.07 Mn 0.10 W 0.001 O2·0.0025Li2B4O7.
[0128] Table 7 The test results of the element mass content of high nickel compound D2 are as follows
[0129] element Li Ni Co Mn W B % 7.453 49.7184 4.2102 5.6069 0.1875 0.1103
[0130] Table 8 Characterization data of high nickel compounds obtained in the examples
[0131]
[0132] As shown in Table 8, the total free lithium
[0133] <1500ppm, specific surface area 0.3-0.9m 2 / g, the particle size is between 3.0-12μm, the FWHM(006) / FWHM(102) ratio is between 1.05 and 1.15, the FWHM(108) / FWHM(110) ratio is between 0.95 and 1.05, the structure and interface are stable, and it is relatively stable in the air.
[0134] It can be seen from Table 8 that in the embodiment, when the Ni molar fraction is 0.83, the capacity of the positive electrode material is 198.1 mAh / g, and the conventional water washing process (Comparative Example 1) is only 191.5 mAh / g, and the cycle is basically the same, but the gas production performance is significantly better. When the nickel molar fraction exceeds 0.9, the capacity can reach 206.2 mAh / g, which provides a basis for the subsequent application of high-nickel compound products. The high-nickel compound and its preparation process proposed in this application make the gas production performance of the positive electrode material better than the performance of the material prepared by the existing process.
[0135] The technical content and technical features of this application have been disclosed as above, but those skilled in the art may still make various substitutions and modifications based on the teachings and disclosures of this application without departing from the spirit of this application. Therefore, the protection scope of this application should not be limited to the contents disclosed in the embodiments, but should include various substitutions and modifications without departing from this application, and be covered by the claims of this application.
Claims
1. A high nickel compound, the general chemical formula of which is Li a Ni x Co y Mn z M b O2·cα·dβ, where 1≤a≤1.2, 0<b≤0.01, 0<c≤0.01, 0<d≤0.02, 0.8≤x≤1, 0≤y<0.12, 0≤z≤0.2, x+y+z=1; M is a doping element; α is a first coating, β is a second coating; wherein the first coating and the second coating process adopt a solvent-free process.
2. The high nickel compound according to claim 1, wherein M is selected from one or more of VB and VIB group elements.
3. The high nickel compound according to claim 1, wherein α is selected from compounds containing one or more elements of Group VB and Group VIB elements.
4. The high-nickel compound according to claim 1, wherein β is selected from one or more of boric acid, lithium borate, lithium metaborate, lithium tetraborate and other boron-containing compounds, or β is formed by one or more of boric acid, lithium borate, lithium metaborate, lithium tetraborate and other boron-containing compounds.
5. The high-nickel compound according to any one of claims 1 to 4, wherein: In the X-ray diffraction spectrum of the high-nickel compound, the ratio of the half-peak width FWHM(006) of the (006) diffraction peak near 37.9° to the half-peak width FWHM(102) of the (102) diffraction peak near 38.2°, FWHM(006) / FWHM(102), is 1.05 to 1.
15.
6. The high-nickel compound according to any one of claims 1 to 4, wherein: In the X-ray diffraction spectrum of the high-nickel compound, the ratio of the half-peak width FWHM(108) of the (108) diffraction peak near 64.3° to the half-peak width FWHM(110) of the (110) diffraction peak near 64.7°, FWHM(108) / FWHM(110), is 0.95 to 1.
05. 7 . A positive electrode sheet, comprising a positive electrode current collector and a positive electrode active material, wherein the positive electrode active material comprises the high-nickel compound according to any one of claims 1 to 6.
8. An electrode assembly comprising: A negative electrode sheet, comprising a negative electrode current collector and a negative electrode active material located on the negative electrode current collector; And the positive electrode sheet according to claim 7.
9. A battery comprising the electrode assembly according to claim 8.
10. An electrical device comprising the battery according to claim 9, wherein the battery is used to provide electrical energy.
11. A method for preparing a high-nickel compound, comprising: (1) mixing a lithium source, a nickel-cobalt-manganese precursor and an M source, and performing a first calcination treatment to prepare a first main material, wherein the M source is a compound containing an element M, and the general formula of the first main material is Li a Ni x Co y Mn z M b O2, 1≤a≤1.2, 0<b≤0.01, 0.8≤x≤1, 0≤y<0.12, 0≤z≤0.2, x+y+z=1; (2) mixing the first main material with a source A and performing a second calcination treatment to prepare a second main material, wherein the source A is a compound containing element A; and (3) mixing the second main material with a B source and performing a third roasting treatment, wherein the B source is a compound containing elemental boron, Wherein, steps (2) and (3) both adopt solvent-free process.
12. The method according to claim 11, wherein: The element M is selected from one or more elements of the VB and VIB groups, and the element A is selected from one or more elements of the VB and VIB groups.