Electrolyte for improving high-rate discharge performance of lithium battery and lithium battery

By using high content of fluoroacetonitrile and lithium tetrafluorooxalate phosphate in lithium battery electrolyte, combined with fluorinated polyetheramine and R-fluorosulfonamide, the problems of insufficient conductivity and attenuation of cyclic properties of traditional electrolytes were solved, and the problem of insufficient circulation performance of traditional electrolytes was achieved. Improved high magnification and low temperature performance.

CN119009123AActive Publication Date: 2024-11-22XIAMEN SHOUNENG TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411084702.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-22
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

The conductivity of traditional lithium battery electrolytes at high and low temperatures is insufficient, which cannot meet the needs of high energy density and high magnification. The existing technology using fluoroacetonitrile as a co-solvent leads to attenuation of battery cycling performance.

Method used

The electrolyte containing 10% to 70% fluoroacetonitrile, 2% to 5% lithium tetrafluorooxalate phosphate, 0.3% to 2% fluorinated polyetheramine and 0.5% to 6% R-fluorosulfonamide were used to pass fluoroacetonitrile and The combination of lithium tetrafluorooxalate phosphate and fluorinated polyetheramine inhibits the negative impact of fluoroacetonitrile on the negative electrode and improves conductivity and cycling performance.

Benefits of technology

It significantly improves the large-rate discharge performance and low-temperature circulation performance of lithium batteries, enhances the conductivity of the electrolyte, and extends the cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides an electrolyte for improving the high-rate discharge performance of a lithium battery and the lithium battery, and relates to the technical field of lithium ion battery materials. The electrolyte comprises a lithium salt, a non-aqueous solvent and an additive, the non-aqueous solvent comprises fluoroacetonitrile, and the additive comprises lithium tetrafluoro oxalate phosphate. By adding the fluoroacetonitrile solvent into the electrolyte, the conductivity of the electrolyte and the high-rate discharge performance of the battery are remarkably improved. In addition, lithium tetrafluoroborate phosphate is added into the electrolyte, so that the negative influence of fluoroacetonitrile on a negative electrode can be inhibited, and the cycle performance of the battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion battery materials, and in particular to an electrolyte and a lithium battery for improving the high-rate discharge performance of a lithium battery. Background Art

[0002] Lithium-ion batteries have gained a dominant position in many fields such as the consumer electronics market, power battery market, and energy storage market due to their advantages such as high energy density, long life, and no memory effect. With the development of the low-altitude economy, the demand for high-rate lithium batteries is increasing day by day. Traditional electrolytes use carbonate solvents or carboxylate solvents, and their conductivity is approximately between 7-13mS / cm. Moreover, the conductivity will drop significantly at low temperatures, which cannot meet the growing demand of consumers for high-energy-density and high-rate lithium batteries.

[0003] Patent CN117996181A discloses a local high-concentration flame-retardant electrolyte. Using 2%-10% fluoroacetonitrile as a diluent can reduce the viscosity of the electrolyte. However, the local high-concentration flame-retardant electrolyte has a low conductivity and cannot meet the requirements of high-rate discharge of the battery. Patent CN117317372B discloses a fluorinated additive electrolyte. The patent claims involve the technology of using fluoroacetonitrile as a co-solvent, but the patent does not disclose technical data on the impact of fluoroacetonitrile on battery performance. In fact, because fluoroacetonitrile has a small molecule, it is easy to undergo a reduction reaction with the negative electrode, resulting in serious degradation of the battery cycle performance. The existing technology using fluoroacetonitrile as a co-solvent is obviously difficult to meet the requirements of high-rate discharge and long cycle performance. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides an electrolyte and a lithium battery for improving the high-rate discharge performance of a lithium battery.

[0005] The present invention solves the technical problem by adopting the following technical solutions.

[0006] A first aspect of the present invention provides an electrolyte for improving the high-rate discharge performance of a lithium battery, comprising: a lithium salt, a non-aqueous solvent and an additive, wherein the non-aqueous solvent comprises fluoroacetonitrile, and the additive comprises lithium tetrafluorooxalate phosphate.

[0007] Further, in a preferred embodiment of the present invention, the mass percentage of the fluoroacetonitrile (FAN) in the electrolyte is 10% to 70%. More preferably, the mass percentage of the fluoroacetonitrile in the electrolyte is 20 to 60%, for example, 20%, 30%, etc. The higher the content of fluoroacetonitrile, the higher the conductivity of the electrolyte, and the higher the high-rate discharge performance of the battery.

[0008] Furthermore, in a preferred embodiment of the present invention, the mass percentage of the lithium tetrafluorooxalate phosphate (LiOTFP) in the electrolyte is 2% to 5%, for example, 2%, 3%, 4%, etc.

[0009] Furthermore, in a preferred embodiment of the present invention, the additives further include fluorinated polyetheramine (F-PEA) and R-fluorosulfonamide (RCONHSO 2 F).

[0010] Specifically, the fluorinated polyetheramine can be prepared by the following method: 1.5 mol hexafluoroisopropanol, 5 mol ethylene glycol dimethyl ether and 0.5 g BF 3 Add to the reaction kettle, slowly drop 10 mol of propylene oxide under the conditions of pressure of 0.10 MPa and temperature of 45°C. After the dropwise addition is completed, react at 70°C for 10 hours, and then vacuum to remove impurities to obtain the reaction product. The reaction product, precious metal catalyst, 5 mol of liquid ammonia and hydrogen are introduced into the reaction equipment. The temperature of the reaction equipment is controlled to be 120°C and the pressure is 2 MPa. After reacting for 24 hours, cool down and filter to obtain the fluorinated polyether amine.

[0011] Specifically, R-fluorosulfonamide can be selected from one or more of the following:

[0012]

[0013] Furthermore, the preparation steps of R-fluorosulfonamide may be: placing carboxylic acid (such as benzoic acid) and fluorosulfonyl isocyanate in acetonitrile, and reacting at room temperature for 5 to 10 hours to obtain R-fluorosulfonamide.

[0014] Furthermore, in a preferred embodiment of the present invention, the mass fraction of the fluorinated polyether amine in the electrolyte is 0.3% to 2%, and the mass fraction of the R-fluorosulfonamide in the electrolyte is 0.5% to 6%. By adding fluorinated polyether amine and R-fluorosulfonamide to the electrolyte, a synergistic effect can be exerted with fluoroacetonitrile to further improve the high-rate discharge performance of the electrolyte. Fluorinated polyether amine and fluorosulfonyl groups can reduce the occurrence of negative electrode side reactions, and can improve the low-temperature storage performance of the electrolyte, reduce the negative electrode film formation impedance, and improve the low-temperature cycle performance.

[0015] Furthermore, in a preferred embodiment of the present invention, the electrolyte also includes an organic solvent, and the organic solvent is selected from one or more of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), propyl acetate (PA) and ethyl propionate (EP).

[0016] Furthermore, in a preferred embodiment of the present invention, the additives further include vinylene carbonate (VC), fluoroethylene carbonate (FEC), 1,3-propane sultone (PS), lithium difluorophosphate (LiPO 2 F 2 ), lithium difluorooxalatoborate (LiDFOB), dithiodisulfate (DTD) and propenyl-1,3-sultone (PST) One or more of.

[0017] Furthermore, in a preferred embodiment of the present invention, the lithium salt is selected from lithium hexafluorophosphate (LiPF 6 ) and lithium bis(fluorosulfonyl)imide (LiFSI) or both.

[0018] Furthermore, in a preferred embodiment of the present invention, the mass fraction of the lithium salt in the electrolyte is 12% to 20%. For example, the content of the lithium salt is 12%, 15%, 18%, etc. Further preferably, the mass fraction of the lithium salt in the electrolyte is 15% to 17%. The higher the content of the lithium salt, the higher the rate performance can be. However, if the content of the lithium salt is too high, the cost of the electrolyte will be too high.

[0019] A second aspect of the present invention provides a lithium battery, comprising the electrolyte as described in any one of the above items, wherein the discharge rate of the lithium battery is above 15C.

[0020] The electrolyte and lithium battery for improving the high-rate discharge performance of lithium batteries according to the embodiments of the present invention have the following beneficial effects:

[0021] The present invention uses fluoroacetonitrile as an electrolyte additive, which can effectively improve the conductivity of the electrolyte, so that the high-rate discharge performance of the battery is effectively improved. Fluoroacetonitrile and lithium tetrafluorooxalate phosphate are compounded for use to inhibit the negative effect of fluoroacetonitrile on the negative electrode, thereby effectively improving the cycle performance of the battery.

[0022] Furthermore, the additives also include fluorinated polyetheramine (F-PEA) and R-fluorosulfonamide (RCONHSO 2 F), by adding fluorinated polyether amine and R-fluorosulfonamide, a synergistic effect can be exerted with fluoroacetonitrile to improve the high-rate discharge performance and low-temperature performance of the battery. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0024] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0025] Example 1

[0026] This embodiment provides an electrolyte with the following formula: 10g LiPF 6 , 7g LiFSI, 25gEC, 22g EMC, 18gEP, 10g FAN, 3g LiOTFP, 1g LiPO 2 F 2 , 1.5g PS, 1.5g VC, 1g DTD; the above components are mixed evenly to obtain a lithium-ion battery electrolyte, named SNA01.

[0027] Example 2

[0028] This embodiment provides an electrolyte with the following formula: 10g LiPF 6 , 7g LiFSI, 25gEC, 17g EMC, 18gEP, 15g FAN, 3g LiOTFP, 1g LiPO 2 F 2 , 1.5g PS, 1.5g VC, 1g DTD; the above components are mixed evenly to obtain a lithium-ion battery electrolyte, the model is named SNA02.

[0029] Example 3

[0030] This embodiment provides an electrolyte with the following formula: 10g LiPF 6 , 7g LiFSI, 25gEC, 12g EMC, 18gEP, 20g FAN, 3g LiOTFP, 1g LiPO 2 F 2 , 1.5g PS, 1.5g VC, 1g DTD; the above components are mixed evenly to obtain a lithium-ion battery electrolyte, the model is named SNA03.

[0031] Example 4

[0032] This embodiment provides an electrolyte with the following formula: 10g LiPF 6 , 7g LiFSI, 25gEC, 7g EMC, 18gEP, 25g FAN, 3g LiOTFP, 1g LiPO 2 F 2 , 1.5g PS, 1.5g VC, 1g DTD; the above components are mixed evenly to obtain a lithium-ion battery electrolyte, the model is named SNA04.

[0033] Example 5

[0034] This embodiment provides an electrolyte with the following formula: 10g LiPF 6 , 7g LiFSI, 20gEC, 2g EMC, 18gEP, 30g FAN, 1g F-PEA, 4g RCONHSO 2 F, 3gLiOTFP, 1g LiPO 2 F 2 , 1.5g PS, 1.5g VC, 1g DTD; the above components are mixed evenly to obtain a lithium-ion battery electrolyte, the model is named SNA05.

[0035] The preparation method of F-PEA is as follows: 1.5 mol hexafluoroisopropanol, 5 mol ethylene glycol dimethyl ether and 0.5 g BF 3 Add to the reaction kettle, slowly drop 10 mol of propylene oxide under the conditions of pressure of 0.10 MPa and temperature of 45°C. After the dropwise addition is completed, react at 70°C for 10 hours, and then vacuum to remove impurities to obtain the reaction product. The reaction product, precious metal catalyst, 5 mol of liquid ammonia and hydrogen are introduced into the reaction equipment. The temperature of the reaction equipment is controlled to be 120°C and the pressure is 2 MPa. After reacting for 24 hours, cool down and filter to obtain the fluorinated polyether amine.

[0036] RCONHSO 2 The structural formula of F is:

[0037]

[0038] Example 6

[0039] This embodiment provides an electrolyte with the following formula: 10g LiPF 6 , 7g LiFSI, 20gEC, 2g EMC, 18gEP, 30g FAN, 5g RCONHSO 2 F (same as Example 5), 3g LiOTFP, 1g LiPO 2 F 2 , 1.5g PS, 1.5g VC, 1g DTD; the above components are mixed evenly to obtain a lithium-ion battery electrolyte, the model is named SNA06.

[0040] Example 7

[0041] This embodiment provides an electrolyte with the following formula: 10g LiPF 6 , 7g LiFSI, 25g EC, 2g EMC, 17g EP, 30g FAN, 1g F-PEA (same as Example 5), 3g LiOTFP, 1g LiPO 2 F 2, 1.5g PS, 1.5g VC, 1g DTD; the above components are mixed evenly to obtain a lithium-ion battery electrolyte, the model is named SNA07.

[0042] Example 8

[0043] This embodiment provides an electrolyte with the following formula: 10g LiPF 6 , 7g LiFSI, 25gEC, 10g EP, 40gFAN, 3g LiOTFP, 1g LiPO 2 F 2 , 1.5g PS, 1.5g VC, 1g DTD; the above components are mixed evenly to obtain a lithium-ion battery electrolyte, the model is named SNA08.

[0044] Example 9

[0045] This embodiment provides an electrolyte with the following formula: 10g LiPF 6 , 7g LiFSI, 25gEC, 50g FAN, 3gLiOTFP, 1g LiPO 2 F 2 , 1.5g PS, 1.5g VC, 1g DTD; the above components are mixed evenly to obtain a lithium-ion battery electrolyte, the model is named SNA09.

[0046] Example 10

[0047] This embodiment provides an electrolyte with the following formula: 10g LiPF 6 , 7g LiFSI, 15gEC, 60g FAN, 3gLiOTFP, 1g LiPO 2 F 2 , 1.5g PS, 1.5g VC, 1g DTD; the above components are mixed evenly to obtain a lithium-ion battery electrolyte, the model is named SNA10.

[0048] Embodiment 11

[0049] This embodiment provides an electrolyte with the following formula: 10g LiPF 6 , 7g LiFSI, 5g EC, 70g FAN, 3gLiOTFP, 1g LiPO 2 F 2 , 1.5g PS, 1.5g VC, 1g DTD; the above components are mixed evenly to obtain a lithium-ion battery electrolyte, the model is named SNA11.

[0050] Example 12

[0051] This embodiment provides an electrolyte with the following formula: 10g LiPF 6 , 7g LiFSI, 20g EC, 17g EMC, 18g EP, 15g FAN, 1.5g F-PEA (same as Example 5), 4.5g RCONHSO 2 F (same as Example 5), 3g LiOTFP, 1g LiDFOB, 1.5g PS, 1.5g VC, 1g DTD; the above components are mixed evenly to obtain a lithium ion battery electrolyte, the model is named SNA12.

[0052] Embodiment 13

[0053] This embodiment provides an electrolyte with the following formula: 10g LiPF 6 , 7g LiFSI, 25gEC, 18g EMC, 18gEP, 15g FAN, 2g LiOTFP, 1g LiPO 2 F 2 , 1.5g PS, 1.5g FEC, 1g DTD; the above components are mixed evenly to obtain a lithium-ion battery electrolyte, the model is named SNA13.

[0054] Embodiment 14

[0055] This embodiment provides an electrolyte with the following formula: 10g LiPF 6 , 7g LiFSI, 25gEC, 16g EMC, 18gEP, 15g FAN, 4g LiOTFP, 1g LiPO 2 F 2 , 1.5g PST, 1.5g FEC, 1g DTD; the above components are mixed evenly to obtain a lithium-ion battery electrolyte, the model is named SNA14.

[0056] Embodiment 15

[0057] This embodiment provides an electrolyte with the following formula: 10g LiPF 6 , 7g LiFSI, 20gEC, 5g PC, 15gEMC, 18g EP, 15g FAN, 5g LiOTFP, 1g LiPO 2 F 2 , 1.5g PS, 1.5g FEC, 1g DTD; the above components are mixed evenly to obtain a lithium-ion battery electrolyte, the model is named SNA15.

[0058] Example 16

[0059] This embodiment provides an electrolyte with the following formula: 10g LiPF6 , 2g LiFSI, 25g EC, 5g PC, 17g EMC, 18g EP, 15g FAN, 3g LiOTFP1g LiDFOB, 1.5g PS, 1.5g VC, 1g DTD; mix the above components evenly to obtain a lithium-ion battery electrolyte, named SNA16.

[0060] Embodiment 17

[0061] This embodiment provides an electrolyte with the following formula: 10g LiPF 6 , 10g LiFSI, 22gEC, 17g EMC, 18gEP, 15g FAN, 3g LiOTFP, 1g LiDFOB, 1.5g PS, 1.5gVC, 1g DTD; the above components are evenly mixed to obtain a lithium-ion battery electrolyte, the model is named SNA17.

[0062] Comparative Example 1

[0063] This comparative example provides an electrolyte with the following formula: 10g LiPF 6 , 7g LiFSI, 25gEC, 25g EMC, 28gEP, 1g LiPO 2 F 2 , 1.5g PS, 1.5g VC, 1g DTD; the above components are mixed evenly to obtain lithium-ion battery electrolyte, the model is named SNB01.

[0064] Comparative Example 2

[0065] This comparative example provides an electrolyte with the following formula: 10g LiPF 6 , 7g LiFSI, 25gEC, 25g EMC, 18gEP, 10g FAN, 1g LiPO 2 F 2 , 1.5g PS, 1.5g VC, 1g DTD; the above components are mixed evenly to obtain a lithium-ion battery electrolyte, the model is named SNB02.

[0066] Test Example 1

[0067] The performance test of the electrolyte was carried out using a lithium cobalt oxide high-rate battery cell for consumer-grade drones. Specifically, the electrolyte samples prepared in the above-mentioned Examples 1 to 17, Comparative Examples 1 and 2 were first tested for their conductivity, and then injected into the dry battery cells that were not injected with liquid, sealed, formed, and divided into volumes, and then the rate performance test and low-temperature performance test were carried out. Three dry battery cells were used for each group of electrolyte injection, and the test results were taken as the average value of the three battery cells.

[0068] The prepared battery was subjected to a 30C high rate discharge test and the discharge retention rate was calculated. The charge cut-off voltage was 4.2V and the discharge cut-off voltage was 2.7V. 30C discharge retention rate = 30C discharge capacity / 1C discharge capacity * 100%, and the results are shown in Table 1.

[0069] Table 1

[0070]

[0071]

[0072] As can be seen from Table 1, as the amount of fluoroacetonitrile added continues to increase, the conductivity of the electrolyte also continues to increase, and the high-rate discharge performance of the battery continues to improve. However, the cost of fluoroacetonitrile is high, so different amounts of fluoroacetonitrile can be added according to the customer's performance and price balance requirements. In addition, the additional addition of fluorinated polyamide and R-fluorosulfonamide can further improve the high-rate discharge performance and low-temperature performance of the electrolyte. From the comparison of Examples 16 and 17, when the lithium salt content (the total content of LiFP6 plus LiFSI) is 12%, the rate performance of the battery will decrease, but it is still better than the performance without fluoroacetonitrile; when the lithium salt content is 20%, the rate performance of the battery will be improved, but a high content of lithium salt will increase the cost of the electrolyte, so an appropriate content of lithium salt (such as 15%-17%) has a higher cost performance.

[0073] Test Example 2

[0074] The battery made of the electrolyte obtained by using Examples 1, 4 and 5 and Comparative Examples 1 and 2 was subjected to a cycle test, and the discharge retention rate after 300 cycles was calculated. The charge cut-off voltage was 4.2V, and the discharge cut-off voltage was 2.7V. The charge rate was 1C, and the discharge rate was 15C. The cycle retention rate after 300 weeks = 300th discharge capacity / first discharge capacity * 100%, and the results are shown in Table 2. The prepared battery was subjected to a 15C high-rate discharge test, and the 15 discharge capacity retention rate was calculated. 15C discharge capacity retention rate = 15C discharge capacity / 1C discharge capacity * 100%, and the results are shown in Table 2.

[0075] Table 2

[0076]

[0077] As can be seen from Table 2, lithium tetrafluorooxalate phosphate can greatly improve the high-rate discharge performance and low-temperature performance of lithium-ion batteries. Using a discharge rate of 15C for testing, fluoroacetonitrile can also greatly improve the high-rate discharge performance and low-temperature performance of the battery. In particular, when fluoroacetonitrile is used in combination with fluorinated polyamide and R-fluorosulfonamide, the high-rate discharge performance of the battery is further improved.

[0078] The embodiments described above are part of the embodiments of the present invention, rather than all of the embodiments. The detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

Claims

1. An electrolyte for improving the high-rate discharge performance of a lithium battery, characterized in that: include: A lithium salt, a non-aqueous solvent and an additive, wherein the non-aqueous solvent comprises fluoroacetonitrile and the additive comprises lithium tetrafluorooxalate phosphate.

2. The electrolyte for improving the high-rate discharge performance of a lithium battery according to claim 1, characterized in that: The mass percentage of the fluoroacetonitrile in the electrolyte is 10% to 70%.

3. The electrolyte for improving the high-rate discharge performance of a lithium battery according to claim 1, characterized in that: The mass percentage of the lithium tetrafluorooxalate phosphate in the electrolyte is 2% to 5%.

4. The electrolyte for improving the high-rate discharge performance of a lithium battery according to claim 1, characterized in that: The additives also include fluorinated polyetheramines and R-fluorosulfonamides.

5. The electrolyte for improving the high-rate discharge performance of a lithium battery according to claim 4, characterized in that: The mass fraction of the fluorinated polyether amine in the electrolyte is 0.3% to 2%, and the mass fraction of the R-fluorosulfonamide in the electrolyte is 0.5% to 6%.

6. The electrolyte for improving the high-rate discharge performance of a lithium battery according to claim 1, characterized in that: The electrolyte further comprises an organic solvent, and the organic solvent is selected from one or more of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, dimethyl carbonate, propyl acetate and ethyl propionate.

7. The electrolyte for improving the high-rate discharge performance of a lithium battery according to claim 1, characterized in that: The additive further comprises one or more of vinylene carbonate, fluoroethylene carbonate, 1,3-propane sultone, lithium difluorophosphate, lithium difluorooxalatoborate, vinyl sulfate and propenyl-1,3-sultone.

8. The electrolyte for improving the high-rate discharge performance of a lithium battery according to claim 1, characterized in that: The lithium salt is selected from one or both of lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide.

9. The electrolyte for improving the high-rate discharge performance of a lithium battery according to claim 1, characterized in that: The mass fraction of the lithium salt in the electrolyte is 12% to 20%.

10. A lithium battery, characterized in that: Comprising the electrolyte according to any one of claims 1 to 9, the discharge rate of the lithium battery is above 15C.

Citation Information

Patent Citations

  • Electrolyte additive, electrolyte and lithium ion battery

    CN116454382A

  • Nonaqueous electrolyte and lithium ion secondary battery

    JP2015118852A

  • Nonaqueous electrolyte solution, and nonaqueous electrolyte secondary battery

    WO2011099585A1