Non-linear optical chromophores having short chain bridged structures, low light loss materials containing them, and methods for their preparation

By designing nonlinear optical chromophores with short-chain bridging groups in electrophotopolymers, the dual problems of high electrophoto activity and time stability in electrophotopolymers are solved, and high transparency, low light loss and high thermal stability are achieved. electro-optical materials suitable for a variety of optical applications.

CN119013616APending Publication Date: 2024-11-22LIGHTWAVE LOGIC INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280087843.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-01-05
Filing Date
2022-12-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art is difficult to achieve nonlinear optical chromophores with high electro-optical activity and time stability in electro-optical polymers, and methods to increase chromophore concentration may reduce polarization efficiency and time stability, limiting the commercial application of materials. .

Method used

Design a nonlinear optical chromophore with short-chain bridging groups between donor and acceptor, reducing the maximum absorption wavelength (λmax) and improving glass transition by optimizing the structure of the chromophore in polar solvents Temperature (Tg) to achieve high thermal stability and maintenance of electro-optical properties.

Benefits of technology

It realizes high transparency, low light loss, higher electro-optical coefficient (r33), abnormally high thermal stability and light stability in a large wavelength range, and is suitable for short-distance local area networks, LED fiber optic communications and terahertz applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013616A_ABST
    Figure CN119013616A_ABST
Patent Text Reader

Abstract

The present invention provides non-linear optical chromophores having a short chain bridging group between a donor and an acceptor, which chromophores exhibit a reduced [lambda] max value and a narrow absorption band. Electro-optical films prepared from the provided non-linear optical chromophores have enhanced transparency to wavelengths outside of a narrow absorption band, as well as low light loss, high thermal stability and high light stability.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of U.S. Provisional Patent Application No. 63 / 296,579, filed on January 5, 2022, the entire contents of which are hereby incorporated by reference. Background Art

[0003] Nonlinear optical (NLO) chromophores provide electro-optic (EO) activity in polarized electro-optic polymer devices. Electro-optic polymers have been studied for many years as a replacement for inorganic materials such as lithium niobate in electro-optic devices. Electro-optic devices can include external modulators for telecommunications, data communications, RF optoelectronics, and optical interconnects, for example. Polymer electro-optic materials have shown great potential for core applications in a wide range of next-generation systems and devices, including electro-optic modulators, optical switches, phased array radars, satellite and fiber-optic communications, cable television (CATV), optical gyroscopes for air and missile guidance, electronic countermeasures (ECM) systems, backplane interconnects for high-speed computing, ultra-fast analog-to-digital conversion, mine detection, RF optoelectronics, spatial light modulation, and all-optical (optically switched light) signal processing.

[0004] Many NLO molecules (chromophores) have been synthesized that exhibit high molecular electro-optical properties. Since the dipole is involved in material processing, the product of the molecular dipole moment (μ) and the hyperpolarizability (β) is usually used as a measure of molecular electro-optical performance. See Dalton et al., "New Class of High Hyperpolarizability Organic Chromophores and Process for Synthesizing the Same", WO 00 / 09613.

[0005] However, the conversion of microscopic molecular hyperpolarizability (β) into macroscopic material hyperpolarizability (χ 2 ) have encountered great difficulties. Molecular subcomponents (chromophores) must be integrated into NLO materials that exhibit (i) high macroscopic nonlinearity and (ii) sufficient temporal, thermal, chemical, and photochemical stability. High electro-optical activity and the stability of the electro-optical activity, also known as "temporal stability", are important for commercially viable devices. The electro-optical activity in electro-optical polymers can be increased by increasing the concentration of nonlinear optical chromophores in the host polymer and by increasing the electro-optical properties of the chromophores. However, some techniques for increasing the chromophore concentration may reduce polarization efficiency and temporal stability. Solving these dual problems simultaneously is considered to be the ultimate obstacle to the widespread commercialization of EO polymers in many devices and systems.

[0006] High material hyperpolarizability (χ 2) is limited by the poor social properties of NLO chromophores. Commercially viable materials must incorporate chromophores with large molecular density and with the necessary molecular moments statistically oriented along a single material axis. To achieve such an organization, the charge transfer (dipole) properties of NLO chromophores are typically exploited by applying an external electric field during material processing, thereby creating localized low-energy conditions that favor non-centrosymmetric orders. Unfortunately, even at moderate chromophore densities, molecules form multi-molecular dipole-bound (centrosymmetric) aggregates that cannot be resolved by realistic field energies. To overcome this difficulty, the integration of antisocial dipolar chromophores into cooperative material architectures is typically achieved by constructing physical barriers (e.g., antistacking steric groups) that restrict proximal intermolecular relationships.

[0007] Therefore, it is generally considered advantageous in the art to prepare materials that exhibit a high glass transition temperature (T g ) containing nonlinear optical chromophores. Materials with high glass transition temperatures show improved thermal stability and maintain their macroscopic electro-optical properties at higher levels than materials with lower glass transition temperatures. It is also advantageous to prepare nonlinear optical chromophores that show desirable macroscopic optical properties, thermal stability, and have a lower wavelength maximum absorption, i.e., λ max . Summary of the invention

[0008] The present invention generally relates to nonlinear optical chromophores having a short chain bridging group between a donor and an acceptor. Various embodiments of the present invention include nonlinear optical chromophores having a short chain bridging group between a donor and an acceptor, the chromophores exhibiting reduced λ max Various embodiments of the present invention include nonlinear optical chromophores having a short-chain bridging group between a donor and an acceptor in a polar solvent, the chromophores exhibiting a lambda of less than or equal to 800 nm. max In some embodiments, the nonlinear optical chromophore exhibits a λ less than or equal to 750 nm. max In other examples, the nonlinear optical chromophore exhibits a λ less than or equal to 700 nm, less than or equal to 650 nm, or less than or equal to 600 nm. max In certain embodiments, the chromophore exhibits a reduced λ max A nonlinear optical chromophore with a short-chain bridging group between the donor and the acceptor can have a value of max In an exemplary embodiment, the nonlinear optical chromophore may have a narrow absorption band below λ, for example, 30-800 nm. maxIn certain other embodiments, the nonlinear optical chromophore is characterized by a λ based on a chromophore analog in a nonpolar solvent. max Δλ max .

[0009] λ outside the range described in this article max The values ​​are compared to the λ of the embodiments described herein. max The value produces a greater transparency range in a large wavelength range. For example, various nonlinear optical chromophore embodiments provide transparency beyond 800nm, which are applied to 1) short-distance local area networks, 2) free-space fiber optic communications and optical interconnects combined with LEDs or semiconductor lasers, and 3) active materials for terahertz (THz) applications. Various embodiments of the present invention include nonlinear optical chromophores with short-chain bridging groups between donors and acceptors, which show reduced light loss and can provide a higher degree of transparency at various wavelengths. In addition, various embodiments of the present invention have the following optimized characteristics: (1) Higher r at various wavelengths 33 (electro-optic coefficient), (2) higher T g (glass transition temperature), (3) exceptionally high thermal stability, and (4) high light stability.

[0010] Various embodiments of the present invention include nonlinear optical chromophores of formula (I):

[0011] D-Π-A(I)

[0012] wherein D represents an organic electron-donating group; A represents an organic electron-accepting group having an electron affinity greater than that of D; and II represents a II bridge between A and D; wherein the II bridge comprises a carbon chain covalently bonded to and separating A and D, wherein the carbon chain length between A and D is 2 to 4 carbon atoms, and wherein the chain of 2 to 4 carbon atoms comprises up to 2 carbon-carbon double bonds and up to 4 side substituents, wherein two or more side substituents may form a ring structure with the chain of 2 to 4 carbon atoms.

[0013] Various embodiments of the present invention include the general formula (I a ) of the nonlinear optical chromophore:

[0014]

[0015] Wherein, D represents an organic electron-donating group; A represents an organic electron-accepting group having an electron affinity greater than that of D; x is 1 or 2; and wherein each R independently represents hydrogen, an alkyl group, an aryl group, an alkyl or aryl group connected to sulfur or oxygen, an aryl group directly connected by a carbon-carbon bond (optionally carrying an adamantane group) (e.g., adamantyl anisole), a halogen, a halogenated alkyl group, a halogenated aryl group, a branched or unbranched C1-C4 substituent optionally containing heteroatoms, or an adamantane-containing group. In various embodiments, one or more R substituents may represent a moiety having 1 to 4 carbon atoms. In various embodiments, one or more R substituents may represent a thiophene moiety.

[0016] In various embodiments of the present invention, the electron donating group comprises a substituted or unsubstituted quinolinyl group. In various embodiments of the present invention, the π bridge comprises a lateral thiophene-containing substituent.

[0017] In certain embodiments, a composition of a nonlinear optical chromophore is provided for use in preparing an electro-optical film exhibiting one or more high optical properties, wherein the nonlinear optical chromophore exhibits a λ less than or equal to 800 nm. max value, and one or more of the high optical properties is the electro-optic coefficient of the electro-optic film. In an exemplary embodiment, the nonlinear optical chromophore has the general formula (1) D-II-A, wherein D represents an organic electron-donating group; A represents an organic electron-accepting group having an electron affinity greater than that of D, and II represents a II bridge between A and D, wherein the II bridge comprises a carbon chain covalently bonded to and separating A and D, wherein the carbon chain length between A and D is 2 to 4 carbon atoms, and wherein the 2 to 4 carbon atom chain comprises up to 2 carbon-carbon double bonds and up to 4 side substituents. In this example and other examples, a high boiling point aprotic polar solvent may be used, wherein the solvent is suitable for promoting a high material hyperpolarizability in the electro-optic film.

[0018] Other aspects, features and advantages will be apparent from the following disclosure including the detailed description, preferred embodiments and the appended claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The foregoing summary of the invention and the following detailed description of preferred embodiments of the present invention will be better understood when read in conjunction with the accompanying drawings. For the purpose of illustrating the present invention, currently preferred embodiments are shown in the accompanying drawings. However, it should be understood that the present invention is not limited to the precise arrangements and means shown.

[0020] In the accompanying drawings,

[0021] Figure 1Spectrum 100 shows the absorption of an exemplary short-chain bridge chromophore of Formula 1a on the UV-Vis spectrum in two different solvents, wherein a first curve 101 shows the absorption of an exemplary short-chain bridge chromophore of Formula 1a on the UV-Vis spectrum in a 1,4-dioxane solvent, and a second curve 102 shows the absorption of an exemplary short-chain bridge chromophore of Formula 1a on the UV-Vis spectrum in a dichloromethane (DCM) solvent.

[0022] Figure 2 Spectrum 200 shows the absorption of the second exemplary short-chain bridge chromophore of Formula 1a on the UV-Vis spectrum in two different solvents, wherein a first curve 201 shows the absorption of the second exemplary short-chain bridge chromophore of Formula 1a on the UV-Vis spectrum in 1,4-dioxane solvent, and a second curve 102 shows the absorption of the second exemplary short-chain bridge chromophore of Formula 1a on the UV-Vis spectrum in dichloromethane (DCM) solvent.

[0023] Figure 3 Spectrum 300 shows the absorption of the third exemplary short-chain bridge chromophore of Formula 1a on the UV-Vis spectrum in two different solvents, wherein a first curve 301 shows the absorption of the third exemplary short-chain bridge chromophore of Formula 1a on the UV-Vis spectrum in 1,4-dioxane solvent, and a second curve 302 shows the absorption of the third exemplary short-chain bridge chromophore of Formula 1a on the UV-Vis spectrum in dichloromethane (DCM) solvent.

[0024] Figure 4 Spectrum 400 shows the absorption of the fourth exemplary short-chain bridge chromophore of Formula 1a on the UV-Vis spectrum in two different solvents, wherein a first curve 401 shows the absorption of the fourth exemplary short-chain bridge chromophore of Formula 1a in 1,4-dioxane solvent on the UV-Vis spectrum, and a second curve 402 shows the absorption of the fourth exemplary short-chain bridge chromophore of Formula 1a in dichloromethane (DCM) solvent on the UV-Vis spectrum.

[0025] Figure 5 Spectrum 500 shows the absorption of the fifth exemplary short-chain bridge chromophore of Formula 1a on the UV-Vis spectrum in two different solvents, wherein a first curve 501 shows the absorption of the fifth exemplary short-chain bridge chromophore of Formula 1a on the UV-Vis spectrum in 1,4-dioxane solvent, and a second curve 502 shows the absorption of the fifth exemplary short-chain bridge chromophore of Formula 1a on the UV-Vis spectrum in dichloromethane (DCM) solvent.

[0026] Figure 6Spectrum 600 shows the absorption of the sixth exemplary short-chain bridge chromophore of Formula 1a on the UV-Vis spectrum in two different solvents, wherein a first curve 601 shows the absorption of the sixth exemplary short-chain bridge chromophore of Formula 1a in 1,4-dioxane solvent on the UV-Vis spectrum, and a second curve 602 shows the absorption of the sixth exemplary short-chain bridge chromophore of Formula 1a in dichloromethane (DCM) solvent on the UV-Vis spectrum.

[0027] Figure 7 Spectrum 700 shows the absorption of the seventh exemplary short-chain bridge chromophore of Formula 1a on the UV-Vis spectrum in two different solvents, wherein a first curve 701 shows the absorption of the seventh exemplary short-chain bridge chromophore of Formula 1a on the UV-Vis spectrum in 1,4-dioxane solvent, and a second curve 702 shows the absorption of the seventh exemplary short-chain bridge chromophore of Formula 1a on the UV-Vis spectrum in dichloromethane (DCM) solvent.

[0028] Figure 8 Spectrum 800 shows the absorption of the eighth exemplary short-chain bridge chromophore of Formula 1a on the UV-Vis spectrum in two different solvents, wherein a first curve 801 shows the absorption of the eighth exemplary short-chain bridge chromophore of Formula 1a in 1,4-dioxane solvent on the UV-Vis spectrum, and a second curve 802 shows the absorption of the eighth exemplary short-chain bridge chromophore of Formula 1a in dichloromethane (DCM) solvent on the UV-Vis spectrum. DETAILED DESCRIPTION

[0029] As used herein, the singular terms "a", "a", and "the" are synonymous and are used interchangeably with "one or more" and "at least one", unless the language and / or context clearly indicate otherwise. Thus, for example, reference to "a polymer" or "the polymer" herein or in the appended claims may refer to a single polymer or more than one polymer. As a further example, reference to "a solvent" or "the solvent" herein or in the appended claims may refer to a single solvent or a mixture of more than one solvent. In addition, unless otherwise specifically stated, all numerical values ​​are understood to be modified by the word "about".

[0030] As used herein, the term "nonlinear optical chromophore" (NLOC) refers to a molecule or portion of a molecule that produces a nonlinear optical effect when illuminated with light. A chromophore is any molecular unit that interacts with light to produce a nonlinear optical effect. The desired effect can occur at resonant or nonresonant wavelengths. The activity of a particular chromophore in a nonlinear optical material is expressed in terms of its hyperpolarizability, which is directly related to the molecular dipole moment of the chromophore. Various embodiments of the NLO chromophores of the present invention are useful structures for producing the NLO effect.

[0031] The first-order hyperpolarisability (β) is one of the most common and useful NLO properties. Higher-order hyperpolarisabilities are useful in other applications such as all-optical (optically switched light) applications. In order to determine whether a material such as a compound or polymer includes a first-order hyperpolarisability and a sufficient electro-optic coefficient (r 33 ) (the electro-optic coefficient is a function of β), the following test can be performed. First, the material in thin film form is placed in an electric field to align the dipoles. For example, this can be done by sandwiching a film of material between electrodes, such as an indium tin oxide (ITO) substrate, a gold film, or a silver film.

[0032] The nonlinear optical chromophores of the embodiments herein have a short-chain bridging group between the donor and the acceptor, and the chromophores exhibit reduced λ max Value, in λ max The nonlinear optical chromophore having a short-chain bridging group between the donor and the acceptor may have a narrow absorption band, for example, below 50-800 nm. max As another example, a nonlinear optical chromophore having a short-chain bridging group between the donor and the acceptor can be formed at λ max It has a narrow absorption band below 30-50nm.

[0033] By calculating the λ of the nonlinear optical chromophore in a standard polar solvent (such as DCM) max Relative to the λ of the analog in nonpolar solvents (such as 1,4-dioxane) max To measure Δλ max The less polar (1,4-dioxane) solvent will stabilize the neutral ground state chromophore, while the more polar solvent (DCM) will stabilize the charge transfer state of the chromophore. The easier the charge transfer occurs, the more "polarizable" the chromophore is, and therefore the more reactive it is. It has been found that higher wavelengths are proportional to lower energies. Therefore, the Δλ between the two solvents is max The higher is the energy required to achieve the charge transfer state, the less energy is needed. In addition, r, which is measured experimentally and is equivalent to the responsiveness of the light passing through to the applied electric field, 33 With Δλmax has a general correlation, where the larger Δλ max Usually with larger r 33 In this way, Δλ max Characterizes the "strength" of the electro-optical activity of a chromophore. For example, Δλ above ~30 nm for chromophores and their analogs max With sufficiently large r 33 Preferably, Δλ max It is above 35nm.

[0034] See also Figure 1 , the absorption of the chromophore (IU4128A) was measured in two different solvents. The concentration of the sample in each solvent was 17 μg / mL. The λ of the chromophore IU4128A max In dichloromethane (DCM), it is 653.45 nm, and in 1,4-dioxane, it is 622.40 nm.

[0035] See also Figure 2 , the absorption of the chromophore (IV8422) was measured in two different solvents. The concentration of the sample in each solvent was 17 μg / mL. The λ of the chromophore IV8422 max The wavelength in dichloromethane (DCM) is 661.97 nm and in 1,4-dioxane is 595.77 nm.

[0036] See also Figure 3 , the absorption of the chromophore (KM4042) was measured in two different solvents. The concentration of the sample in each solvent was 17 μg / mL. max 662 nm in dichloromethane (DCM), and λ max In 1,4-dioxane it is 627 nm.

[0037] See also Figure 4 , the absorption of the chromophore (KM4043) was measured in two different solvents. The concentration of the sample in each solvent was 17 μg / mL. max 630 nm in dichloromethane (DCM), and λ max In 1,4-dioxane it is 596 nm.

[0038] See also Figure 5 , the absorption of the chromophore (KM4044) was measured in two different solvents. The concentration of the sample in each solvent was 17 μg / mL. max 617 nm in dichloromethane (DCM), and λ max In 1,4-dioxane it is 581 nm.

[0039] See also Figure 6, the absorption of the chromophore (KM4051) was measured in two different solvents. The concentration of the sample in each solvent was 17 μg / mL. max 661 nm in dichloromethane (DCM), and λ max In 1,4-dioxane it is 626 nm.

[0040] See also Figure 7 , the absorption of the chromophore (KM4060) was measured in two different solvents. The concentration of the sample in 1,4-dioxane was 14 μg / mL, while the concentration of the sample in dichloromethane (DCM) was 8.5 μg / mL. max 631 nm in dichloromethane (DCM), and λ max In 1,4-dioxane it is 595 nm.

[0041] See also Figure 8 , the absorption of the chromophore (KM4084) was measured in two different solvents. The concentration of the sample in each solvent was 17 μg / mL. max 627 nm in dichloromethane (DCM), and λ max In 1,4-dioxane it is 593 nm.

[0042] Figure 1-8 The short-chain bridge chromophore λ max and Δλ max The data is summarized as follows:

[0043] Chromophore <![CDATA[λ max DCM]]> <![CDATA[λ max 1,4-Dioxane]]> <![CDATA[Δλ max ]]> IU4128A 653nm 622nm 31nm IV8422 662nm 596nm 66nm KM4042 662nm 627nm 35nm KM4043 630nm 596nm 34nm KM4044 617nm 581nm 36nm KM4051 661nm 626nm 35nm KM4060 631nm 595nm 36nm KM4084 627nm 593nm 34nm

[0044] Then, to generate the polarization field, an electric potential is applied to the electrodes while the material is heated to near its glass transition (T g ) temperature. After a suitable period of time, the temperature is gradually reduced while maintaining the polarizing electric field. Alternatively, the material can be polarized by a corona poling method, in which a charged needle at a suitable distance from the material film provides a polarizing electric field. In either case, the dipoles in the material tend to align with the field. Various embodiments according to the present invention may include or may also include an electro-optical material having a material glass transition temperature greater than or equal to 100°C, greater than or equal to 125°C, or greater than or equal to 150°C, or even higher.

[0045] The nonlinear optical properties of the polarized material are then tested as follows. Polarized light, typically from a laser, is passed through the polarized material and then through a polarizing filter to a light intensity detector. If the intensity of the light received at the detector changes as a function of the potential applied to the electrodes, then the material has incorporated a nonlinear optical chromophore and has an electro-optically variable refractive index. A more detailed discussion of techniques for measuring the electro-optic constants of polarized films that have incorporated nonlinear optical chromophores can be found in Chia-Chi Teng, Measuring Electro-Optic Constants of aPoled Film, in Nonlinear Optics of Organic Molecules and Polymers, Chapter 7, pp. 447-49 (Hari Singh Nalwa & Seizo Miyata, eds., 1997), which is incorporated by reference in its entirety, except in the case of disclosures or definitions that are inconsistent with this application, in which case the disclosures or definitions herein shall be deemed valid.

[0046] The relationship between the change in applied potential and the change in the refractive index of a material can be expressed in terms of its electro-optical (EO) coefficient (r 33 ) is represented. This effect is generally referred to as the electro-optical effect or EO effect. Devices that include materials that change their refractive index in response to changes in applied potential are referred to as electro-optical (EO) devices. For the compositions described herein with short-chain bridge chromophores, high EO coefficients of >30 pm / V (e.g. measured at 980 nm) or >20 pm / V (e.g. measured at 1310 nm) can be achieved.

[0047] The compositions described herein with short-chain bridge chromophores can also show reduced light loss. The light loss of various described embodiments can be <2dB / cm. In addition, the compositions described herein can provide a higher degree of transparency at wavelengths outside the absorption bands of various embodiments herein. In addition, the compositions described herein can also show unusually high thermal stability, characterized in that the decomposition temperature is greater than 250°C, and high light stability measured by degradation of light-optical materials under broad-band light and environmental conditions.

[0048] The second-order hyperpolarizability (γ) or the third-order susceptibility (χ (3) ) is a standard measure of third-order NLO activity. Although there are several methods for measuring these properties, degenerate four-wave mixing (DFWM) is very common. See CW Thiel, "For-wave Mixing and Its Applications," www.physics.montana.edu.students.thiel.do cs / FWMixing.pdf, the entire contents of which are hereby incorporated by reference. Referring to published U.S. patent application No. US2012 / 0267583A1, the entire contents of which are hereby incorporated by reference, a method for evaluating the third-order NLO properties of thin films can be used, which is known in the art as Degenerate Four Wave Mixing (DFWM). Figure 4 In this figure, beams 1 and 2 are picosecond coherent pulses that are absorbed by the NLO film deposited on the glass substrate. Beam 3 is a weaker, slightly delayed beam with the same wavelength as beams 1 and 2. Beam 4 is the product of wave mixing, diffracted by the temporal holographic grating, resulting from the interference of beams 1 and 2 in the NLO material of the film. Beam 3 can be a "control" beam at a telecommunications wavelength that produces a "signal" beam of a certain frequency that is not absorbed by the NLO material.

[0049] Nonlinear optical chromophores suitable for use according to various embodiments of the present invention include those having the general formula (I):

[0050] D-Π-A(I)

[0051] Wherein, D represents an organic electron-donating group; A represents an organic electron-accepting group having an electron affinity greater than that of D; and II represents an II bridge between A and D. The terms electron-donating group (donor or "D"), II bridge (bridging group or "II"), and electron-accepting group (acceptor or "A") according to the various embodiments described herein and general synthetic methods for forming D-II-A chromophores are known in the art, for example, as described in U.S. Patent Nos. 5,670,091, 5,679,763, 6,090,332, and 6,716,995 and U.S. Patent Application No. 17 / 358,960 filed on June 25, 2021, the entire contents of each of which are incorporated herein by reference.

[0052] Acceptor is an atom or atom group with low reduction potential, wherein the atom or atom group can accept electrons from a donor through a π-bridge. Acceptor (A) has a higher electron affinity than a donor (D), therefore, at least in the absence of an external electric field, the chromophore is usually polarized in the ground state, and the electron density on the acceptor (D) is relatively high. Generally, the acceptor group contains at least one electronegative heteroatom as a part of a π bond (double bond or triple bond), so that the electron pair of the π bond can be formed to move to the heteroatom and simultaneously reduce the multiplicity of the π bond (that is, the double bond is formally converted to a single bond or the triple bond is formally converted to a double bond) resonance structure, so that the heteroatom obtains a formal negative charge. The heteroatom can be a part of a heterocycle. Exemplary acceptor groups include but are not limited to-NO2,--CN,--CHO, COR, CO2R,--PO(OR)3,--SOR,--SO2R and--SO3R, wherein R is an alkyl, aryl or heteroaryl. The total number of heteroatoms and carbons in the acceptor group is about 30, and the acceptor group may be additionally substituted with alkyl, aryl and / or heteroaryl groups.

[0053] Suitable electron accepting groups "A" (also referred to in the literature as electron withdrawing groups) of the nonlinear optical chromophore that can be used according to various embodiments of the present invention include those described in the following published U.S. patent applications: US2007 / 0260062; US2007 / 0260063; US 2008 / 0009620; US2008 / 0139812; US2009 / 0005561; US 2012 / 0267583A1 (collectively, “Prior Publications”), each of which is incorporated herein by reference in its entirety; and those described in the following U.S. Patent Nos.: 6,584,266; 6,393,190; 6,448,416; 6,44,830; 6,514,434; 5,044,725; 4,795,664; 5,247,042; 5,196,509; 4,810,338; 4,936,645; 4,767,169; 5,326,661; 5,187,234; 5,170,461; 5,133,037; 5,106,211; and 5,006,285; each of which is also incorporated herein by reference in its entirety.

[0054] Among the nonlinear optical chromophores suitable for use in various embodiments according to the present invention, suitable electron accepting groups may include those according to the general formula (II a )

[0055]

[0056] Where R 2 and R 3Each independently represents a structural moiety selected from the group consisting of: H, substituted or unsubstituted C1-C 10 Alkyl, substituted or unsubstituted C2-C 10 Alkenyl, substituted or unsubstituted C2-C 10 alkynyl, substituted or unsubstituted aryl, substituted or unsubstituted alkylaryl, substituted or unsubstituted carbocyclic ring, substituted or unsubstituted heterocyclic ring, substituted or unsubstituted cyclohexyl and (CH2) n -O-(CH2) n , wherein n is 1-10. As used herein, In various preferred embodiments, R 2 and R 3 One or both represent halogen-substituted moieties. Halogen substitution may refer to mono-, di-, tri- and higher degrees of substitution. In various embodiments, R 2 and R 3 One of them represents a halogen-substituted alkyl moiety and the other represents an aromatic moiety. In various embodiments, R 2 and R 3 One of them represents a halogen-substituted aromatic moiety and the other represents an alkyl moiety. In various embodiments, the electron accepting group can be

[0057]

[0058] In various embodiments, the electron accepting group can be

[0059]

[0060] In various embodiments, the electron accepting group can be

[0061]

[0062] Donor includes an atom or atom group with low oxidation potential, wherein the atom or atom group can provide electrons for acceptor "A" through a π bridge. Donor (D) has a lower electron affinity than acceptor (A), therefore, at least in the absence of an external electric field, the chromophore is usually polarized, and the electron density on the donor (D) is relatively low. Generally, the donor group contains at least one heteroatom, and the heteroatom has a lone pair of electrons that can be conjugated with the p orbital of the atom directly connected to the heteroatom, so that the lone pair of electrons can be formed to move to the p orbital key of the atom directly connected to the heteroatom, so as to formally increase the multiplicity of the bond between the heteroatom and the atom directly connected to the heteroatom (that is, a single bond is formally converted to a double bond or a double bond is formally converted to a triple bond) resonance structure, so that the heteroatom obtains a formal positive charge. The p orbital of the atom directly connected to the heteroatom can be empty or can be a part of a multiple bond with another atom except the heteroatom. The heteroatom can be a substituent of an atom with a π bond or can be in a heterocycle. Exemplary donor groups include, but are not limited to, R2N— and R n X 1 --, where R is an alkyl, aryl or heteroaryl group, X 1 is O, S, P, Se or Te, and n is 1 or 2. The total number of heteroatoms and carbons in the donor group may be about 30, and the donor group may be additionally substituted with alkyl, aryl or heteroaryl groups.

[0063] Suitable electron donating groups "D" (also referred to in the literature as electron withdrawing groups) of nonlinear optical chromophores that can be used according to various embodiments of the present invention include those described in the following published U.S. patent applications: US2007 / 0260062; US2007 / 0260063; US 2008 / 0009620; US2008 / 0139812; US2009 / 0005561; US ​​2012 / 0267583A1 (collectively, "Prior Publications"), each of which is incorporated herein by reference in its entirety; and those described in the following U.S. Patent Nos.: 6,584,266; 6,393,190; 6,448,416; 6,44,830; 6,514,434; 5,044,725; 4,795,664; 5,247,042; 5,196,504. 9; 4,810,338; 4,936,645; 4,767,169; 5,326,661; 5,187,234; 5,170,461; 5,133,037; 5,106,211; and 5,006,285; and U.S. patent application No. 17 / 358,960 filed on June 25, 2021, each of which is also incorporated herein by reference in its entirety.

[0064] In various embodiments, the electron donating group may include a quinolyl group, which may be substituted or unsubstituted, including hydrogen and alkyl substituents, aryl substituents, and combinations thereof. Such a quinolyl group may have one or more adamantane groups covalently attached thereto. For example, the electron donating group may include alkoxyphenyl substituted quinolones, such as:

[0065] or for example aromatic nitrogen-containing groups such as:

[0066]

[0067] A "π bridge" includes atoms or groups of atoms through which electrons can be delocalized from an electron donor (as defined above) to an electron acceptor (as defined above) via an atomic orbital in the bridge. Such groups are well known in the art. Typically, the orbitals will be bi(sp 2 In some embodiments, the chromophore of the present invention is a chromophore of the present invention. The ...

[0068] According to various embodiments of the nonlinear optical chromophore disclosed herein, the π bridge includes a carbon chain separating an electron donating group from an electron accepting group, wherein the length of the chain separating the two is 2 to 4 carbon atoms. The π bridge may additionally include one or more side substituents, the atoms of the side substituents being not included in the chain length count. In various embodiments, two or more side substituents may form a ring structure having a 2 to 4 carbon atom bridge. For example, the π bridge in the nonlinear optical chromophore according to various embodiments of the present invention may include a carbon chain according to the general formula (I a )-(I h ), wherein A, D, x and each R are as defined above in this document:

[0069]

[0070]

[0071] The nonlinear optical chromophores according to various embodiments of the present invention exhibit a maximum absorption (λ) of ≤ 800 nm. max). The nonlinear optical chromophores according to various embodiments of the present invention exhibit excellent second-order optical properties and have excellent thermal stability. The nonlinear optical chromophores according to various embodiments of the present invention may be used in admixture with one or more host polymers or matrix materials, and / or one or more solvents, or may be used in pure form (i.e., without a host polymer or solvent). The nonlinear optical chromophores according to various embodiments of the present invention may be formed into thin films for electro-optical devices and polarized according to various methods known in the art for use in producing ordered thin films.

[0072] The invention will now be described in more detail with reference to the following non-limiting examples.

[0073] Example

[0074] Example 1: Chromophore IU4128A

[0075] Synthesis of triphenyl(p-tolyl)silane:

[0076]

[0077] A dry RB flask (1) was charged with 1-bromo-4-methyl-benzene (9.93 mL, 0.0807 mol) and THF (200 mL), then cooled in a dry ice / acetone bath to -78°C. n-Butyl lithium (2.50 mol / L, 32.3 mL, 0.0807 mol) was added at a rate (5 mL increments) such that the temperature did not rise above -55°C, and the reaction was stirred at -78°C for 2 hours under nitrogen.

[0078] Another RB flask (2) was evacuated, then filled with nitrogen 3 times, charged with triphenylsilyl chloride (26.2 g, 0.0888 mol), evacuated / filled with nitrogen 3 times, and stirred under vacuum for 1 H at 60° C. The flask (2) was cooled, filled with nitrogen, then charged with THF (100 mL) and cooled to −78° C.

[0079] The contents of flask 2 were introduced into flask 1 in a steady drip, raising the temperature by 5° C. The reaction was stirred under nitrogen and allowed to slowly warm to room temperature.

[0080] The reaction was diluted with DCM, washed with water then brine, dried over MgSO4 and evaporated to give a white solid which was stirred in hexanes for 1 h and filtered / washed with hexanes (500 mL).

[0081] Triphenyl(p-tolyl)silane (25.4 g, 0.0725 mol, yield: 89.8%) was obtained as a white powder.

[0082] Wohl-Ziegler bromination of triphenyl(p-tolyl)silane:

[0083]

[0084] A RB flask was charged with triphenyl(p-tolyl)silane (0 mmol / L, 0 mL, 0.0394 mol), N-bromosuccinimide (7.36 g, 0.0413 mol), 400 mL of DCM and 2-[(E)-(1-cyano-1-methyl-ethyl)azo]-2-methyl-propionitrile (0.323 g, 0.00197 mol). The reaction was refluxed overnight under nitrogen. TLC indicated quantitative conversion to the bromide. The reaction was washed with water, then brine, dried over MgSO4, and evaporated to give a tan powder. This was triturated in hexanes and filtered to give 13.8 g of the first fraction, and the filtrate was evaporated to give 3.49 g of the second fraction. The hexane fraction was chromatographed, eluting with hexanes / ethyl acetate (3-5%). The appropriate fractions were combined and evaporated to give a very white granular powder, 885 mg.

[0085] [4-(Bromomethyl)phenyl]-triphenyl-silane (14.7 g, 0.0342 mol, yield: 87.0%) was obtained.

[0086] Alkylation of 2,2,4,7-tetramethyl-3,4-dihydro-1H-quinoline:

[0087]

[0088] Under nitrogen, a RB flask was charged with [4-(bromomethyl)phenyl]-triphenyl-silane (13.8 g, 0.0321 mol), 2,2,4,7-tetramethyl-3,4-dihydro-1H-quinoline (6.08 g, 0.0321 mol) and 200 mL of DMF. The mixture was cooled to 0°C and sodium hydride (60.0%, 1.41 g, 0.0353 mol) was then added. The reaction was stirred under nitrogen and slowly warmed to RT. At 2H, the reaction had warmed and was uniform, and after about 15 minutes the product crashed out and stirring was stopped. The reaction became a white paste that looked like a solid.

[0089] The reaction was triturated in water then filtered / washed with water. The organics were chromatographed eluting with hexane / ethyl acetate (5%). The appropriate fractions were combined and evaporated to give an off-white solid. This was dissolved in DCM, hexane was added and the DCM was evaporated. The resulting solid was filtered.

[0090] Triphenyl-[4-[(2,2,4,7-tetramethyl-3,4-dihydroquinolin-1-yl)methyl]phenyl]silane (10.86 g, 0.0202 mol, yield: 63.0%) was obtained.

[0091] Vilsmeier-Haack formylation of triphenyl-[4-[(2,2,4,7-tetramethyl-3,4-dihydroquinolin-1-yl)methyl]phenyl]silane:

[0092]

[0093] Under nitrogen, 200mL DCM, N,N-dimethylformamide (3.69mL, 0.0479mol) and POCl3 (4.04mL, 0.0442mol) were loaded into a round-bottomed flask. The reaction was stirred for 1 hour, and then quinoline (dissolved in another 200mL DCM) was added to the reaction at a fast drop rate via a dropping funnel. The mixture was stirred at room temperature for 16hr, and then stirred for another 24hr at 32°C. The reaction mixture was cooled to room temperature, 10% sodium carbonate was then added, and the reaction was stirred vigorously for 1 hour. Each phase was separated, and organic matter was dried over anhydrous MgSO4. Raw material was purified by silica gel column elution (using DCM as eluent). Appropriate fractions were combined and concentrated. The resulting material was ground in hexane, filtered and dried.

[0094] 2,2,4,7-Tetramethyl-1-[(4-triphenylsilylphenyl)methyl]-3,4-dihydroquinoline-6-carbaldehyde (18.9 g, 0.0334 mol, yield: 90.7%) was obtained as a bluish white powder.

[0095] Knoevenagel Condensation:

[0096]

[0097] A round bottom flask was charged with 2,2,4,7-tetramethyl-1-[(4-triphenylsilylphenyl)methyl]-3,4-dihydroquinoline-6-carbaldehyde (1.00 g, 0.00177 mol), 2-[3-cyano-4-methyl-5-(4-phenylphenyl)-5-(trifluoromethyl)-2-furylidene]malononitrile (0.692 g, 0.00177 mol), 1-propanol (10.0 mL) and acetic acid (1.01 mL, 0.0177 mol). The reaction was sealed and stirred at 80 °C for 16 hr. The reaction mixture was removed from the heating and evaporated. The residue was purified by normal phase chromatography (eluted with 15-30% EtOAc in hexane). The appropriate fractions were combined and evaporated to give a colored film. It was dissolved in DCM and crystallized overnight by evaporation.

[0098] 2-[3-Cyano-5-(4-phenylphenyl)-4-[(E)-2-[2,2,4,7-tetramethyl-1-[(4-triphenylsilylphenyl)methyl]-3,4-dihydroquinolin-6-yl]vinyl]-5-(trifluoromethyl)-2-furylidene]malononitrile (1.12 g, 0.00119 mol, yield: 67.5%) was obtained.

[0099] Example 2: Chromophore IV8422

[0100] Buchwald coupling of 1,2,3,4-tetrahydroquinoline with 1-(5-bromo-2-methoxy-phenyl)adamantane:

[0101]

[0102] A solution of 1,2,3,4-tetrahydroquinoline (2.00 g, 0.0150 mol) and 1-(5-bromo-2-methoxy-phenyl)adamantane (97.0%, 5.22 g, 0.0158 mol) in 50 mL of toluene was purged with N2 and then treated with potassium tert-butoxide (2.19 g, 0.0195 mol), Pd(OAc)2 (0.135 g, 0.000601 mol) and tri-tert-butylphosphine (0.243 g, 0.00120 mol). The flask was equipped with a condenser and the reaction mixture was heated to 115 °C overnight. The reaction mixture was concentrated and then diluted with 1:1 DCM / hexane. The solids were removed by vacuum filtration. The filtrate was concentrated and then diluted with MeOH. A beige solid precipitated from the solution. The solid was separated and then soaked in MeOH (x2) again. The solid was separated and dried by vacuum filtration and then soaked in Et2O (x3). The solid was isolated and dried by vacuum filtration and then air dried over a weekend.

[0103] 1-[3-(1-adamantyl)-4-methoxy-phenyl]-3,4-dihydro-2H-quinoline (96.0%, 5.25 g, 0.0135 mol, yield: 89.8%) was obtained as a tan solid.

[0104] Vilsmeier-Haack Formylation of 1-[3-(1-adamantyl)-4-methoxy-phenyl]-3,4-dihydro-2H-quinoline

[0105]

[0106] A suspension of 1-[3-(1-adamantyl)-4-methoxy-phenyl]-3,4-dihydro-2H-quinoline (96.0%, 4.00 g, 0.0103 mol) and N,N-dimethylformamide (3.98 mL, 0.0514 mol) in DCM (50 mL) was purged with N2 and then treated with dropwise addition of POCl3 (3.76 mL, 0.0411 mol). The mixture was stirred at room temperature. It quickly turned olive green and then after 20 minutes it turned dark amber. After 35 minutes, LCMS analysis showed >99% conversion to imine and aldehyde. The reaction was quenched by pouring into an ice-cold 10% Na2CO3 solution. The mixture was diluted with DCM and stirred vigorously overnight. The DCM had evaporated, leaving an aqueous phase with a large amount of precipitated solids. The solid was collected by vacuum filtration and LCMS analysis showed complete hydrolysis to the aldehyde. The solid was triturated with Et2O (twice) and then separated and dried under vacuum.

[0107] 1-[3-(1-adamantyl)-4-methoxy-phenyl]-3,4-dihydro-2H-quinoline-6-carbaldehyde (98.0%, 4.45 g, 0.0109 mol, yield: 106%) was obtained as a tan solid.

[0108] Wittig condensation of 1-[3-(1-adamantyl)-4-methoxy-phenyl]-3,4-dihydro-2H-quinoline-6-carbaldehyde with thiophenephosphonium bromide:

[0109]

[0110] A solution of triphenyl(2-thienylmethyl)phosphonium bromide (9.74 g, 0.0222 mol) in THF (250 mL) was treated with potassium tert-butoxide (2.49 g, 0.0222 mol). The mixture immediately turned red-orange. After 10 min, 1-[3-(1-adamantyl)-4-methoxy-phenyl]-3,4-dihydro-2H-quinoline-6-carbaldehyde (4.45 g, 0.0111 mol) was added in batches. The flask was capped and the reaction mixture was stirred at room temperature. It almost immediately turned from red-orange to dark red. LCMS analysis after 2 hours showed complete conversion. The mixture was concentrated and the residue was then dissolved in Et2O. The solid was removed by filtration and the filtrate was concentrated. The substance was purified by normal phase chromatography (15% EtOAc in hexane). The product fractions were concentrated.

[0111] 1-[3-(1-adamantyl)-4-methoxy-phenyl]-6-[(E)-2-(2-thienyl)vinyl]-3,4-dihydro-2H-quinoline (87.0%, 5.01 g, 0.00906 mol, yield: 81.7%) was obtained as a bright yellow film.

[0112] Vilsmeier-Haack Formylation of 1-[3-(1-adamantyl)-4-methoxy-phenyl]-6-[(E)-2-(2-thienyl)vinyl]-3,4-dihydro-2H-quinoline

[0113]

[0114] A solution of 1-[3-(1-adamantyl)-4-methoxy-phenyl]-6-[(E)-2-(2-thienyl)vinyl]-3,4-dihydro-2H-quinoline (87.0%, 5.01 g, 0.00906 mol) and DMF (3.51 mL, 0.0453 mol) in DCM (250 mL) was purged with N2 and then treated with dropwise POCl3 (1.04 mL, 0.0113 mol). The bright yellow mixture was stirred at room temperature overnight. The reaction was quenched by pouring into an ice-cold 10% Na2CO3 solution. The mixture was diluted with DCM and stirred vigorously for 96 hr. The DCM was evaporated, leaving an aqueous phase with a large amount of precipitated solids. The solids were collected by vacuum filtration. The solids were dissolved in Et2O and then purified by NP chromatography (20% EtOAc in hexane). The product fractions were concentrated.

[0115] (Z)-3-[1-[3-(1-adamantyl)-4-methoxy-phenyl]-3,4-dihydro-2H-quinolin-6-yl]-2-(2-thienyl)prop-2-enal was obtained as a bright orange solid (96.4%, 2.81 g, 0.00531 mol, yield: 58.7%).

[0116] Knoevenagel condensation of (Z)-3-[1-[3-(1-adamantyl)-4-methoxy-phenyl]-3,4-dihydro-2H-quinolin-6-yl]-2-(2-thienyl)prop-2-enal with 2-(3-cyano-4,5,5-trimethyl-2-furylidene)malononitrile:

[0117]

[0118] A suspension of (Z)-3-[1-[3-(1-adamantyl)-4-methoxy-phenyl]-3,4-dihydro-2H-quinoline-6-yl]-2-(2-thienyl)prop-2-enal (96.4%, 1.00 g, 0.00189 mol) in 50 mL of EtOH was treated with 2-(3-cyano-4,5,5-trimethyl-2-furylidene)malononitrile (0.414 g, 0.00208 mol). The flask was sealed with a septum and the mixture was stirred at 60 ° C for 120 hr. It was then heated to 95 ° C for another 48 hr. The reaction mixture was concentrated and then purified by normal phase chromatography (50-100% DCM in hexane). The product fractions were concentrated and the residue was then recrystallized from DCM / MeOH.

[0119] Green powdery 2-[4-[(1E,3Z)-4-[1-[3-(1-adamantyl)-4-methoxy-phenyl]-3,4-dihydro-2H-quinolin-6-yl]-3-(2-thienyl)buta-1,3-dienyl]-3-cyano-5,5-dimethyl-2-furylidene]malononitrile (0.472 g, 0.000683 mol, yield: 36.1%) was obtained.

[0120] Those skilled in the art will appreciate that changes may be made to the embodiments described above without departing from the broad inventive concept. Therefore, it should be understood that the present invention is not limited to the specific embodiments disclosed, but is intended to cover modifications within the spirit and scope of the present invention as defined by the appended claims.

Claims

1. A composition for preparing an electro-optical film exhibiting one or more optimized optical properties, the composition comprising a nonlinear optical chromophore of formula (I) and a polar solvent suitable for promoting a high material hyperpolarizability in the electro-optical film: D-Π-A(I) in, D represents an organic electron donating group; A represents an organic electron accepting group having an electron affinity greater than that of D; and II represents a II bridge between A and D; wherein the II bridge comprises a carbon chain covalently bonded to and separating A and D, wherein the carbon chain length between A and D is 2 to 4 carbon atoms, and wherein the chain of 2 to 4 carbon atoms comprises up to 2 carbon-carbon double bonds and up to 4 pendant substituents; wherein the nonlinear optical chromophore exhibits a lambda value less than or equal to 800 nm, and wherein the nonlinear optical chromophore exhibits a Δλ greater than or equal to 30 nm compared to an analog in a nonpolar solvent max value.

2. The composition of claim 1, wherein the one or more high optical properties is a high level of transparency at wavelengths greater than 800 nm.

3. The composition of claim 1, wherein the one or more high optical properties is a high electro-optic coefficient, wherein the coefficient value is greater than 20 pm / V when measured at a wavelength greater than or equal to 1000 nm.

4. The composition of claim 1, wherein the one or more high optical properties is a glass transition temperature above about 100°C.

5. The composition of claim 1, wherein the one or more high optical properties is low optical loss, wherein the low optical loss is less than 2 dB / cm.

6. The composition of claim 1, wherein the one or more high optical properties is high thermal stability characterized by a decomposition temperature greater than 250°C.

7. The composition of claim 1, wherein the one or more high optical properties is high photostability as measured by degradation of the electro-optical film under broad-band light and environmental conditions.

8. The composition of claim 1, wherein the nonlinear optical chromophore comprises a nonlinear optical chromophore of formula (Ia): in, D represents an organic electron-donating group; A represents an organic electron-accepting group having an electron affinity greater than that of D; x is 1 or 2; and wherein each R independently represents hydrogen, an alkyl group, an aryl group, an alkyl or aryl group linked to sulfur or oxygen, an aryl group directly linked via a carbon-carbon bond (optionally carrying an adamantane group) (e.g., adamantyl anisole), a halogen, a halogenated alkyl group, a halogenated aryl group, a branched or unbranched C1-C4 substituent optionally containing a heteroatom, or an adamantane-containing group.

9. The nonlinear optical chromophore of claim 8, wherein the electron donating group comprises a substituted or unsubstituted quinolyl group.

10. The nonlinear optical chromophore according to claim 8, wherein the electron donating group is selected from the group consisting of:

11. The nonlinear optical chromophore of claim 8, wherein at least one R group represents a thiophene.

12. The nonlinear optical chromophore of claim 8, wherein x is 2, and wherein at least one R group represents a thiophene.

13. The nonlinear optical chromophore of claim 8, wherein x is 1, and wherein each R represents hydrogen.

14. The nonlinear optical chromophore of claim 9, wherein at least one R group represents a thiophene.

15. The nonlinear optical chromophore of claim 9, wherein x is 2, and wherein at least one R group represents a thiophene.

16. The nonlinear optical chromophore of claim 9, wherein x is 1, and wherein each R represents hydrogen.

17. The composition of claim 1, wherein the nonlinear optical chromophore comprises a nonlinear optical chromophore having the following general formula:

18. The composition of claim 1, wherein the nonlinear optical chromophore comprises a nonlinear optical chromophore having the following general formula: