Method for manufacturing silicon nitride film on substrate having ground

By using a silicon nitride composition in the manufacturing of electronic devices and performing light irradiation heating, the defects of the silicon nitride film in the groove structure are solved, the density and resistance of the film are improved, and the manufacturing efficiency is improved.

CN119013764APending Publication Date: 2024-11-22MERCK PATENT GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380033990.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-18
Filing Date
2023-04-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the manufacturing of electronic devices, the existing silicon nitride films are prone to joints and pore defects in the groove structure, have low density, poor chemical liquid resistance, and are difficult to effectively fill grooves with high aspect ratio, resulting in low manufacturing efficiency.

Method used

By using a method containing a silicon nitride composition, the composition layer is irradiated with light at a wavelength of 200 to 229 nm and heated in a non-oxidizing atmosphere to form a silicon nitride film. The method includes applying a silicon nitride composition on a substrate having grooves, irradiating light and heating, to form a silicon nitride film having high density and chemical liquid resistance.

Benefits of technology

It effectively suppresses the occurrence of defects in the silicon nitride film, improves the density and chemical liquid resistance of the bottom of the groove, and can efficiently fill the grooves with high aspect ratios, improving the device manufacturing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013764A_ABST
    Figure CN119013764A_ABST
Patent Text Reader

Abstract

A method for manufacturing a silicon nitride film on a substrate having a groove, comprising the steps of: (a) applying a silicon nitride composition on the substrate having the groove to form a composition layer; (b) irradiating the composition layer with light having a wavelength of 200 to 229 nm; and (c) heating the substrate in a non-oxidizing atmosphere; wherein the silicon nitride film has a refractive index of 1.70 to 2.40 with respect to light having a wavelength of 633 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a silicon nitride film on a substrate having grooves. Background Art

[0002] Silicon nitride films are generally used as dielectric films or sacrificial films in the manufacture of electronic devices, especially semiconductor devices. Silicon nitride films have been conventionally formed by CVD (chemical vapor deposition) or ALD (atomic layer deposition).

[0003] In the field of electronic devices, device specifications are becoming increasingly refined, and it is necessary to form silicon nitride films in finer groove structures. As refinement progresses, more defects are generated when forming the film, resulting in a problem of reduced manufacturing efficiency of electronic devices. In particular, the generation of seam defects (hereinafter referred to as seams) or pore defects during film formation has become a problem.

[0004] Therefore, it is proposed to form a silicon nitride film using a liquid composition containing a silicon-containing polymer. For example, a method for forming a silicon nitride stress layer is proposed, which is formed by filling a groove with a liquid composition containing polysilazane and then heating it at a high temperature in a nitrogen atmosphere (Patent Document 1).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent document 1: US2009 / 0289284 A1 Summary of the invention

[0008] Technical Problems to be Solved by the Invention

[0009] The present inventors believe that there are still one or more issues that need to be improved in the method of manufacturing a silicon nitride film on a substrate having grooves. Examples of these issues include the following:

[0010] When forming the silicon nitride film, defects such as seams and pores occur; the density of the silicon nitride film at the bottom of the groove is low; the silicon nitride film has low resistance to chemical liquids; it is impossible to efficiently fill grooves with a high aspect ratio; the film quality of the silicon nitride film still has room for improvement; and the manufacturing efficiency of the device is low.

[0011] Solutions for solving technical problems

[0012] The method of manufacturing a silicon nitride film on a substrate having a groove of the present invention comprises the following steps:

[0013] (a) applying a silicon nitride composition on a substrate having a groove to form a composition layer;

[0014] (b) irradiating the composition layer with light having a wavelength of 200 to 229 nm; and

[0015] (c) heating the substrate in a non-oxidizing atmosphere,

[0016] The refractive index of the silicon nitride film for light with a wavelength of 633 nm is 1.70 to 2.40.

[0017] The method for manufacturing an electronic device of the present invention comprises the above method.

[0018] Effects of the Invention

[0019] According to the present invention, one or more of the following effects can be achieved.

[0020] It can suppress the occurrence of defects when forming a silicon nitride film; the density of the silicon nitride film is high even at the bottom of the groove; the silicon nitride film has high resistance to chemical liquids; it can efficiently fill grooves with a high aspect ratio; the film quality of the silicon nitride film is improved; and the manufacturing efficiency of the device is high. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is an electron microscope photograph of Example 3 after applying hydrofluoric acid.

[0022] Figure 2 This is an electron microscope photograph of Comparative Example 1 after application of hydrofluoric acid. DETAILED DESCRIPTION

[0023] Modes for Carrying Out the Invention

[0024] [definition]

[0025] In this specification, unless otherwise specified or mentioned, the definitions and examples described in this paragraph shall apply.

[0026] The singular includes the plural, and “a” and “the” mean “at least one.” An element of a certain concept may be expressed in a plurality of types, and when the amount (eg, mass % or mol %) thereof is described, the amount means the total of the plurality of types.

[0027] "And / or" includes all combinations of elements and also includes individual uses.

[0028] When "to" or "-" is used to express a numerical range, both endpoints are included and the unit is the same. For example, 5 to 25 mol% means 5 mol% or more and 25 mol% or less.

[0029] An alkyl group refers to a group obtained by removing any hydrogen from a straight-chain, branched-chain or cyclic saturated hydrocarbon, including straight-chain alkyl, branched-chain alkyl and cyclic alkyl, and may contain a straight-chain or branched-chain alkyl as a side chain in a cyclic structure as required. An aryl group refers to a group obtained by removing any hydrogen from an aromatic hydrocarbon.

[0030] “C x-y ”, “C x ~C y ” and “C x " refers to the number of carbon atoms in a molecule or substituent. For example: C 1-6 The alkyl group refers to an alkyl chain having 1 to 6 carbon atoms (such as methyl, ethyl, propyl, butyl, pentyl, and hexyl).

[0031] When the polymer has multiple repeating units, these repeating units are copolymerized. These copolymerizations can be alternating copolymerization, random copolymerization, block copolymerization, graft copolymerization, or any of these mixed forms. When the polymer or resin is represented by a structural formula, n, m, etc. recorded outside the brackets represent the number of repetitions.

[0032] The unit of temperature is Celsius. For example, 20 degrees means 20 degrees Celsius.

[0033] The additive refers to the compound itself having the function (for example, if it is a base generator, it is the compound itself that generates the base). It can also be a method in which the compound is dissolved or dispersed in a solvent and added to the composition. As one embodiment of the present invention, these solvents are preferably contained in the composition of the present invention as a solvent or other components.

[0034] The following describes in detail the embodiments of the present invention.

[0035] <Method for producing silicon nitride film>

[0036] The method of the present invention for producing a silicon nitride film on a substrate having a groove includes the following steps.

[0037] (a) applying a silicon nitride composition on a substrate having a groove to form a composition layer;

[0038] (b) irradiating the composition layer with light having a wavelength of 200 to 229 nm; and

[0039] (c) Heating the substrate in a non-oxidizing atmosphere.

[0040] Process (a)

[0041] Step (a) is a step of applying a silicon nitride composition on a substrate having a groove to form a composition layer.

[0042] In the present invention, the substrate may be a single layer or a laminate. The shape of the groove is not particularly limited. Since the present invention has the characteristics of being easy to penetrate even in a narrow groove and forming a uniform silicon nitride film inside the groove, a substrate having a groove or hole with a high aspect ratio is preferred. The shape of the groove is not particularly limited, and the cross section may be any shape such as a rectangle, a positive cone, an inverted cone, a curved surface, etc. In addition, the two ends of the groove may be open or closed.

[0043] The depth of the groove is preferably 150 to 500 nm, more preferably 180 to 500 nm. In one embodiment of the present invention, for a groove deeper than 500 nm, a silicon nitride film can be formed by performing steps (a) to (c) once and then performing steps (a) to (c) again.

[0044] The ratio of the depth of the groove to the width of the groove, that is, the aspect ratio, is preferably 10-100, more preferably 15-50.

[0045] As the substrate having grooves, there can be cited, for example, a substrate for electronic devices having transistor elements, bit lines, capacitors, etc. The production of such electronic devices includes a step of forming an insulating film between a transistor element and a bit line, between a transistor element and a capacitor, between a bit line and a capacitor, or between a capacitor and a metal wiring, or forming an insulating film between a plurality of metal wirings, or burying an isolation groove, and sometimes includes a through-hole forming step of forming a hole that penetrates vertically from the burying material of the fine groove after a step of forming an insulating film between a transistor element and a bit line, or between a transistor element and a capacitor, or between a capacitor and a metal wiring, which is called a PMD, or forming an insulating film between a plurality of metal wirings, or burying an isolation groove.

[0046] The silicon nitride composition is applied to the grooves of the substrate. The application method is not particularly limited, and examples thereof include common coating methods such as spin coating, dipping, spraying, transfer, and slit coating.

[0047] Preferred silicon nitride compositions will be described later.

[0048] When the silicon nitride composition is applied to form a composition layer, a drying step such as spin drying, reduced pressure, prebaking, etc. may be performed as necessary.

[0049] In a preferred embodiment, the method further comprises, before step (b), heating the substrate having the composition layer formed thereon at 70 to 300° C., preferably 75 to 250° C. (prebaking).

[0050] Process (b)

[0051] Step (b) is a step of irradiating the composition layer with light having a wavelength of 200 to 229 nm.

[0052] The wavelength of the irradiation light is preferably 200 to 226 nm. In a preferred embodiment of the present invention, the irradiation light is a KrCl excimer lamp that emits ultraviolet light with a peak wavelength of 222 nm. The illumination is not particularly limited, but is preferably 2 to 80 mW / cm 2 , more preferably 4 to 50 mW / cm 2 The irradiation dose is preferably 4 to 100 J / cm 2 , more preferably 7 to 80 J / cm 2 .

[0053] The substrate may be heated during irradiation with light, but the temperature is preferably 200° C. or lower, more preferably 100° C. or lower, and further preferably the substrate is not heated.

[0054] The atmosphere during light irradiation is not particularly limited, but a non-oxidizing atmosphere is preferred.

[0055] It is considered that condensation between polymers occurs due to light irradiation in this step, and the molecular weight of the polymer increases.

[0056] Process (c)

[0057] Step (c) is a step of heating the light-irradiated substrate in a non-oxidizing atmosphere.

[0058] The heating temperature in this step is preferably 400 to 1,200° C., more preferably 400 to 1,100° C. The heating time is preferably 1 minute to 10 hours, more preferably 1 to 180 minutes.

[0059] The heating atmosphere is a non-oxidizing atmosphere. A non-oxidizing atmosphere refers to an atmosphere with an oxygen concentration of 1% or less and a dew point of -20°C or less. Preferably, it is an atmosphere of N2, Ar, He, Ne, H2, or a mixed gas atmosphere of two or more of these, and more preferably, it is an N2 atmosphere.

[0060] After step (c), the composition layer becomes a silicon nitride film. A silicon nitride film refers to a film containing nitrogen atoms and silicon atoms, wherein the ratio of the number of nitrogen atoms to the number of silicon atoms (N / Si) is 0.68 to 1.1, preferably 0.70 to 1.0, and may contain other atoms such as carbon, hydrogen and oxygen, and also includes a silicon carbonitrogenous film.

[0061] The refractive index of the silicon nitride film with respect to light of a wavelength of 633 nm is 1.70 to 2.40, preferably 1.76 to 2.20, and more preferably 1.78 to 2.20.

[0062] According to the method of the present invention, a substrate having a silicon nitride film in a groove has a uniform and dense silicon nitride film formed in the entire groove. In particular, a uniform and dense film quality is achieved even at the bottom of the groove. As a result, the resistance to chemical liquids is improved, especially the resistance to hydrofluoric acid is high.

[0063] The method for manufacturing an electronic device of the present invention comprises the above method. The electronic device is preferably a semiconductor device, a solar cell chip, an organic light emitting diode, an inorganic light emitting diode, and more preferably a semiconductor device.

[0064] [Silicon nitride composition]

[0065] The silicon nitride composition (hereinafter also referred to as a composition) used in the present invention is not particularly limited as long as it contains a component capable of forming a silicon nitride film.

[0066] When measured with a capillary viscometer at 25° C., the viscosity of the silicon nitride composition is preferably 0.55 to 1.80 mPa·s, more preferably 0.55 to 1.70 mPa·s, and even more preferably 0.57 to 1.60 mPa·s.

[0067] (Silicon-containing polymer)

[0068] The composition of the present invention preferably comprises a silicon-containing polymer selected from polysilazanes, polycarbosilazanes and mixtures thereof.

[0069] The mass average molecular weight of the silicon-containing polymer is preferably 1,000 to 30,000, more preferably 2,000 to 30,000, and even more preferably 3,000 to 30,000. In the present invention, the mass average molecular weight is a mass average molecular weight converted to polystyrene and can be measured by gel permeation chromatography using polystyrene as a standard. The same applies to other polymers.

[0070] In order to prevent the gasification of low molecular weight components and suppress the volume change when filling fine grooves, the more the content of the silicon-containing polymer, the better. On the other hand, for excellent coating properties and good filling of grooves with high aspect ratios, low viscosity is preferred. For these reasons, the content of the silicon-containing polymer is preferably 0.1 to 40% by mass, more preferably 0.2 to 30% by mass, based on the total mass of the composition. Without being bound by theory, by being within the above-mentioned content range of the silicon-containing polymer, the coating film formed in the groove can be suppressed from shrinking during heating to cause low density at the bottom of the groove, and is effective for the high density of the silicon nitride film at the bottom of the groove.

[0071] (Polysilazane)

[0072] The structure of the polysilazane used in the present invention is not particularly limited and can be selected arbitrarily according to the purpose. Polysilazane has Si-N bonds as the main skeleton, and can be any of an inorganic compound or an organic compound, and can be linear, branched, or partially cyclic.

[0073] The polysilazane preferably contains 20 or more, preferably 20 to 350 repeating units selected from the group consisting of the following formulae (1-i) to (1-vi). In this case, the repeating units are preferably directly bonded without interposing repeating units other than (1-i) to (1-vi).

[0074]

[0075] In the formula, R 1a ~R 1i are independently hydrogen, or C 1-4 alkyl.

[0076] It is further preferred that the polysilazane used in the present invention is perhydropolysilazane (hereinafter referred to as PHPS). PHPS is a silicon-containing polymer that contains Si-N bonds as repeating units and is composed only of Si, N and H. In addition to the Si-N bonds, the elements bonded to Si and N in this PHPS are all H, and substantially no other elements such as carbon or oxygen are contained. The simplest structure of perhydropolysilazane is a chain structure having the following repeating units.

[0077]

[0078] The structure of PHPS is not limited as long as it is a silicon-containing polymer containing Si-N bonds as repeating units and consisting only of Si, N and H, and various structures other than those exemplified above may be adopted. PHPS preferably has a cyclic structure or a cross-linked structure, and particularly preferably has a cross-linked structure.

[0079] The mass average molecular weight of the polysilazane is preferably 1,000 to 30,000, more preferably 2,000 to 25,000, and even more preferably 3,000 to 20,000, from the viewpoint of solubility in a solvent and reactivity.

[0080] (Polycarbosilazane)

[0081] The structure of the polycarbosilazane used in the present invention is not particularly limited and can be arbitrarily selected according to the purpose. The polycarbosilazane has a C-Si-N structure as a main skeleton and preferably contains a repeating unit represented by the following formula (2-i) and a repeating unit represented by the following formula (2-ii).

[0082]

[0083] in,

[0084] R 2a , R 2b and R 2c are each independently a single bond, hydrogen, or C 1-4 Alkyl, preferably a single bond or hydrogen.

[0085] R 2d , R 2e and R 2f Each independently is a single bond or hydrogen. Provided that, in R 2a , R 2b , R 2d and R 2e When it is a single bond, it is bonded to N contained in other repeating units. 2c and R 2f In the case of a single bond, it bonds to Si contained in other repeating units.

[0086] n and m are each independently 1 to 3, preferably 1 or 2, and more preferably 1.

[0087] The polycarbosilazane is preferably perhydropolycarbosilazane. 2a , R 2b and R 2c is a single bond or hydrogen, and except for (CH2) of formula (2-i) n and (CH2) m A polymer having no hydrocarbon group other than 1,2-dihydrocarbon.

[0088] The terminal group of the polycarbosilazane is preferably -SiH3.

[0089] The polycarbosilazane of the present invention is preferably substantially composed of a repeating unit represented by formula (2-i) and a repeating unit represented by formula (2-ii). In the present invention, "substantially" means that 95% by mass or more of all structural units contained in the polycarbosilazane are repeating units represented by formula (2-i) and repeating units represented by formula (2-ii). It is further preferred that the polycarbosilazane does not contain repeating units other than the repeating units represented by formula (2-i) and the repeating units represented by formula (2-ii).

[0090] The mass average molecular weight of the polycarbosilazane of the present invention is preferably 1,000 to 25,000, more preferably 2,000 to 20,000.

[0091] (Solvent)

[0092] The composition used in the present invention may contain a solvent. The solvent is selected from a solvent that allows each component contained in the composition to be uniformly dissolved or dispersed. Specifically, examples of the solvent include ethylene glycol monoalkyl ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, and ethylene glycol monobutyl ether; diethylene glycol dialkyl ethers such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, and diethylene glycol dibutyl ether; ethylene glycol alkyl ether acetates such as ethylene glycol monomethyl ether acetate and ethylene glycol monoethyl ether acetate; propylene glycol monoalkyl ethers such as propylene glycol monomethyl ether (PGME) and propylene glycol monoethyl ether propylene glycol alkyl ether acetates such as propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monoethyl ether acetate, and propylene glycol monopropyl ether acetate, aromatic hydrocarbons such as benzene, toluene, xylene, and 1,3,5-trimethylbenzene, ethers such as propylene glycol dimethyl ether, dipropyl ether, dibutyl ether, and anisole, ketones such as methyl ethyl ketone, acetone, methyl amyl ketone, methyl isobutyl ketone, and cyclooctanone, alcohols such as isopropyl alcohol and propylene glycol, alicyclic hydrocarbons such as cyclooctane and decalin, etc. Preferred are xylene, dibutyl ether, and propylene glycol dimethyl ether.

[0093] These solvents may be used alone or in combination of two or more thereof. The content of the solvent is preferably 60 to 99.9% by mass, more preferably 70.0 to 99.8% by mass, based on the total mass of the composition.

[0094] The composition used in the present invention can be further combined with optional components as needed. As optional components, for example, surfactants can be cited. The content of optional components other than the solvent in the entire composition is preferably 10% by mass or less, more preferably 5% by mass or less, and further preferably 1% by mass or less relative to the mass of the whole composition. In one embodiment of the present invention, the composition used in the present invention does not contain components other than the silicon-containing polymer and the solvent.

[0095] [Example]

[0096] The present invention is described below by way of examples. These examples are for illustration purposes only and are not intended to limit the scope of the present invention.

[0097] [Synthesis Example 1: Synthesis of polysilazane 1]

[0098] After replacing the interior of a 10L reaction container equipped with a condenser, a mechanical stirrer and a temperature control device with dry nitrogen, 7,500 ml of dry pyridine was added to the reaction container and cooled to 0°C. Next, 500 g of dichlorosilane was added to generate a white solid adduct (SiH2Cl2·2C5H5N). After confirming that the reaction mixture has dropped below 0°C, 350 g of ammonia was slowly blown into it while stirring. After continuing to stir for 30 minutes, dry nitrogen was blown into the liquid layer for 30 minutes to remove excess ammonia. Under a dry nitrogen atmosphere, the obtained slurry product was pressure filtered using a 0.2 μm filter paper made of Teflon (registered trademark) to obtain 6,000 ml of filtrate. Pyridine was distilled off using an evaporator, and dibutyl ether was added to obtain a 20.4% by mass dibutyl ether solution of polysilazane 1. Filtering was performed using a 0.05 μm filter paper made of Teflon to obtain a silicon nitride composition. The mass average molecular weight (hereinafter referred to as Mw) of the obtained polysilazane 1 was measured by gel permeation chromatography (GPC) and was found to be 1,580 in terms of polystyrene.

[0099] GPC was measured using Alliance (trademark) e2695 high-speed GPC system (manufactured by Nihon Waters KK) and SuperMultipore HZ-N GPC column (manufactured by Tosoh Corporation). The measurement was performed using monodisperse polystyrene as a standard sample and chloroform as a developing solvent under the measurement conditions of a flow rate of 0.6 ml / min and a column temperature of 40°C, and the mass average molecular weight was calculated as the relative molecular weight relative to the standard sample.

[0100] The same measurement method is applied to the following Mw.

[0101] [Synthesis of Intermediate (A)]

[0102] After replacing the interior of a 10L reaction container equipped with a condenser, a mechanical stirrer and a temperature control device with dry nitrogen, 7,500 ml of dry pyridine was added to the reaction container and cooled to -3°C. Next, 500 g of dichlorosilane was added to generate a white solid adduct (SiH2Cl2·2C5H5N). After confirming that the reaction mixture has dropped below -3°C, 350 g of ammonia was slowly blown into it while stirring. After continuing to stir for 30 minutes, dry nitrogen was blown into the liquid layer for 30 minutes to remove excess ammonia. Under a dry nitrogen atmosphere, the obtained slurry product was pressure filtered with a 0.2μm filter paper made of Teflon to obtain 6,000 ml of filtrate. Pyridine was distilled off using an evaporator, and xylene was added to obtain a xylene solution of 39.8% by mass of polysilazane. The Mw of the obtained polysilazane is 1,220. Hereinafter, the polysilazane obtained using this recipe will be referred to as intermediate (A).

[0103] [Synthesis Example 2: Synthesis of polysilazane 2]

[0104] After replacing the interior of a 10L reaction container equipped with a condenser, a mechanical stirrer and a temperature control device with dry nitrogen, 4700g of dry pyridine, 150g of dry xylene and 1650g of the above-obtained 39.8% by mass intermediate (A) were added to the reaction container, and nitrogen was bubbled at 0.5NL / min while being stirred evenly. Next, a modification reaction was carried out at 100°C for 10.5 hours to obtain polysilazane 2. The Mw of polysilazane 2 is 3,200. After distilling off the xylene, dibutyl ether was added to obtain a 19.8% by mass dibutyl ether solution of polysilazane 2. Filtering was performed with a 0.05μm filter paper made of Teflon to obtain a silicon nitride composition. The relative value (R(SiH 1,2 )) is 0.245, and the relative value of the amount of NH (R(NH)) based on the aromatic ring hydrogen of xylene is 0.058.

[0105] [Synthesis Example 3: Synthesis of polysilazane 3]

[0106] In Synthesis Example 2, the conditions of the reforming reaction were changed to 110°C and 10.5 hours, and synthesis was performed to obtain a 19.2% by mass dibutyl ether solution of polysilazane 3. The solution was filtered using a 0.05 μm filter paper made of Teflon to obtain a silicon nitride composition. The Mw of polysilazane 3 was 8,600, and R(SiH 1,2 ) is 0.198, and R(NH) is 0.043.

[0107] [Synthesis Example 4: Synthesis of polycarbosilazane]

[0108] After replacing the interior of a 1L reaction container equipped with a condenser, a mechanical stirrer and a temperature control device with dry nitrogen, 500 ml of dry pyridine was added to the reaction container and cooled to -3°C. Next, 12.3 g of dichlorosilane and 2.75 g of 1,1,3,3-tetrachloro-1,3-disilacyclobutane were added. After confirming that the reaction mixture had dropped below 0°C, 11.3 g of ammonia was slowly blown into it while stirring. After continuing for 30 minutes, dry nitrogen was blown into the liquid layer for 30 minutes to remove excess ammonia. The obtained slurry-like product was pressure filtered with a 0.2 μm filter paper made of Teflon to obtain 400 ml of filtrate. After distilling off the pyridine in the filtrate, xylene was added to obtain a 19.2% by mass xylene solution of polycarbosilazane. Filter with a 0.05 μm filter paper made of Teflon to obtain a silicon nitride composition. The Mw of polycarbosilazane is 5,400.

[0109] [Example 1]

[0110] The silicon nitride composition of polysilazane 1 obtained in Synthesis Example 1 was dropped onto a silicon wafer (8 inches) with a pattern (groove with a width of 20 nm, a length of 2 mm, and a depth of 500 nm), and spin-coated at a rotation speed of 1000 rpm to form a coating. The coating was pre-baked on a hot plate under the conditions of 80°C / N2 / 3 minutes to dry the coating. The excimer 222nm irradiation unit MEUTA-1-200-222-M (MDCOM inc) was used for irradiation for 30 minutes at 222nm and an illumination of 50 mW / cm 2 The irradiated film was annealed at 450℃ / N2 / 60 minutes to obtain a silicon nitride film. The Fourier transform infrared spectroscopy showed that the film -1 A peak was identified at , and from Rutherford backscattering analysis, the N / Si ratio was 0.78 and the refractive index was 1.78, which showed that the obtained film was a silicon nitride film.

[0111] In the evaluation of the resistance of the groove bottom to hydrofluoric acid, no joints or voids were confirmed.

[0112] [Examples 2 to 6 and Comparative Examples 1 and 2]

[0113] A silicon nitride film was obtained by performing the same operation as in Example 1 except that the silicon nitride composition, the wavelength of the irradiation light, and the annealing conditions were changed as described in Tables 1-1 and 1-2. The evaluation results are summarized in Tables 1-1 and 1-2.

[0114] [Table 1-1]

[0115]

[0116] [Table 1-2]

[0117]

[0118] [Refractive index]

[0119] The refractive index was measured at a wavelength of 633 nm at room temperature in the air using a spectroscopic ellipsometer M-2000V (manufactured by JA Woollam Co., Inc.).

[0120] [Fourier Transform Infrared Analysis]

[0121] The measurement was performed by a transmission method at room temperature using a Fourier transform infrared spectrometer FTIR-6600FV (manufactured by JASCO Corporation).

[0122] [Rutherford Backscattering Analysis]

[0123] The N / Si ratio was measured by elemental analysis using Pelletron 3SDH (manufactured by National Electrostatics Corporation) by Rutherford backscattering spectrometry.

[0124] [Resistance of the groove bottom to hydrofluoric acid]

[0125] The annealed pattern substrate was split perpendicularly to the groove direction, immersed in an aqueous solution containing 0.05 mass % hydrofluoric acid for 30 seconds, washed with pure water and dried, and then observed with a scanning electron microscope Regulus 8230 (manufactured by Hitachi High-Tech Fielding Corporation) and evaluated according to the following standards. The electron microscope photographs of the grooves observed in Example 3 and Comparative Example 1 are: Figure 1 and Figure 2 . Figure 1 No joints or pores were confirmed, and it was found that a dense film was formed in the groove. Figure 2 It is found that the groove portion has no resistance to hydrofluoric acid and voids are formed.

[0126] A: No seams or voids were confirmed at the bottom of the groove.

[0127] B: A seam or a void was confirmed at the bottom of the groove.

[0128] C: Clear seams or gaps were confirmed at the bottom of the groove.

Claims

1. A method for producing a silicon nitride film on a substrate having a groove, comprising the following steps: (a) applying a silicon nitride composition on a substrate having a groove to form a composition layer; (b) irradiating the composition layer with light having a wavelength of 200 to 229 nm; and (c) heating the substrate in a non-oxidizing atmosphere, in, The refractive index of the silicon nitride film with respect to light of a wavelength of 633 nm is 1.70 to 2.

40.

2. The method according to claim 1, wherein: The depth of the groove is 150 to 500 nm.

3. The method according to claim 1 or 2, wherein: The silicon nitride composition comprises a silicon-containing polymer selected from polysilazane, polycarbosilazane and a mixture thereof.

4. The method according to claim 3, wherein: The mass average molecular weight of the silicon-containing polymer is 1,000 to 30,000.

5. The method according to any one of claims 1 to 4, wherein: The silicon nitride composition further comprises a solvent.

6. The method according to claim 5, wherein: The content of the silicon-containing polymer is 0.1 to 40% by mass based on the total amount of the silicon nitride composition.

7. The method according to any one of claims 1 to 6, wherein: The viscosity of the silicon nitride composition measured at 25° C. by a capillary viscometer is 0.55 to 1.80 mPa·s.

8. The method according to any one of claims 1 to 7, wherein: Prior to step (b), the method further comprises heating the substrate having the composition layer formed thereon at 70 to 300°C.

9. The method according to any one of claims 1 to 8, wherein: The heating in the step (c) is performed at 400 to 1,200°C. 10 . A substrate having a silicon nitride film in a groove, obtained by the method according to claim 1 .