Composite coating as well as preparation method and application thereof
By using composite coatings of N-Cl type haloamine, copper-based nanoenzyme and cerium oxide on the dental implant surface, the problem of insolidity of existing antibacterial coatings is solved, and the long-term antibacterial effect and excellent performance of bone binding is achieved, thus improving the survival rate of dental implants.
Patent Information
- Application Number
- CN202411149304.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-26
AI Technical Summary
The antibacterial coating on the surface of existing dental implants is not firm, making it difficult to achieve long-term antibacterial effects, resulting in early infection and shedding of dental implants and affecting survival rate.
A composite coating of N-Cl type haloamine coating, copper-based nanoenzyme coating and cerium oxide coating arranged in sequence from bottom to top is prepared by atomic layer deposition method to ensure the stability and antibacterial properties of the coating.
Without affecting the implant bone binding, efficient antibacterials against Staphylococcus aureus and E. coli are achieved, and the survival rate and osseobin capacity of dental implants are improved.
Smart Images

Figure CN119015512A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of antibacterial materials, and in particular relates to a composite coating and a preparation method and application thereof. Background Art
[0002] In recent years, artificial dental implants have become the preferred restoration method for patients with missing or missing teeth. Currently, a major problem facing dental implants is the uncontrolled bacterial growth on the surface of the implants during long-term use, which causes the soft and hard tissues around the implants to shrink and eventually lead to implant loss. Among dental implants that have been used for more than 5 years, the incidence of peri-implantitis caused by bacterial growth is as high as 20-47%, which has become the primary cause of dental implant failure, resulting in a large waste of manpower, financial resources, and material resources.
[0003] In response to peri-implantitis, scholars have made research progress in the prevention and control of early implant infection by performing antibacterial modification on the implant surface, reducing bacterial adhesion and inhibiting biofilm formation. However, the antibacterial coating on the titanium surface through non-covalent adsorption (such as hydrogen bonding and electrostatic interactions) is not strong, and the antibacterial components may be rapidly degraded from the surface after implantation in the body. On the other hand, traditional chemical coating methods usually involve the application of antibiotics and antimicrobial peptides to the modified titanium surface, and the antibacterial effect decreases rapidly over time. Therefore, it is difficult for existing methods to achieve the long-term antibacterial goals required for dental implants, and there is an urgent need to improve the long-lasting antibacterial properties of the implant surface and improve the survival rate of dental implants.
[0004] Nanozymes are a new type of nanoparticle-based catalytic enzymes. Compared with traditional natural enzymes, nanozymes have significant advantages such as simple preparation, low cost, easy large-scale production and high stability. Copper-based nanozymes (CuO NPs) induce the body to produce a controllable reactive oxygen storm by releasing copper ions, and have become a research hotspot in the field of biological antibacterial in recent years. In the slightly acidic environment of anaerobic bacteria, CuO NPs express peroxidase activity, which catalyzes the decomposition of hydrogen peroxide inside the bacteria into hydroxyl radicals, causing fatal oxidative stress to the bacteria. In a neutral physiological environment, CuO NPs express catalase activity, avoiding the damage of oxidative stress to normal tissues. However, due to the high reactivity of reactive oxygen and the limited diffusion distance in the environment, high concentrations of metal oxides are cytotoxic, and directly using them as implant surface coatings will affect implant bone bonding. There are technical barriers to directly applying copper-based nanozymes to implant antibacterial coatings. Therefore, how to use copper-based nanozymes in implant antibacterial coatings without affecting implant bone bonding has become a technical problem that needs to be solved in this field. Summary of the invention
[0005] The purpose of the present invention is to provide a composite coating and a preparation method and application thereof. The composite coating provided by the present invention does not affect the bone integration of the implant and has excellent antibacterial properties.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The invention provides a composite coating, comprising an N-Cl type halamine coating, a copper-based nanozyme coating and a cerium oxide coating which are sequentially stacked from bottom to top.
[0008] Preferably, the thickness of the N-Cl type halamine coating is 1 to 5 nm.
[0009] Preferably, the thickness of the copper-based nanozyme coating is 3 to 200 nm.
[0010] Preferably, the thickness of the cerium oxide coating is 5 to 50 nm.
[0011] The present invention also provides a method for preparing the composite coating according to the above technical solution, which is characterized by comprising the following steps:
[0012] (1) preparing an N-Cl type halamine coating on the surface of a substrate;
[0013] (2) preparing a copper-based nanozyme coating on the upper surface of the N-Cl type halamine coating obtained in step (1) by atomic layer deposition;
[0014] (3) A cerium oxide coating is prepared on the upper surface of the copper-based nanozyme coating obtained in step (2) by atomic layer deposition to obtain a composite coating.
[0015] Preferably, the atomic layer deposition methods in step (2) and step (3) are independently performed in atomic layer deposition equipment.
[0016] Preferably, the process of preparing the copper-based nanozyme coating by atomic layer deposition comprises the following steps:
[0017] 1) introducing a copper precursor into an atomic layer deposition device, and then performing a first surface chemical adsorption reaction to obtain an N-Cl type halamine coating adsorbed with the copper precursor;
[0018] 2) introducing an oxygen precursor into an atomic layer deposition device, and then performing a first oxidation reaction to obtain a single-layer copper-based nanozyme coating;
[0019] 3) Repeat the operations of steps 1) and 2) to obtain a copper-based nanozyme coating.
[0020] Preferably, the time for introducing the copper precursor in step 1) is 1 to 5 seconds.
[0021] Preferably, the process of preparing the cerium oxide coating by atomic layer deposition comprises the following steps:
[0022] I. introducing a cerium precursor into an atomic layer deposition device, and then performing a second surface chemical adsorption reaction to obtain a copper-based nanozyme coating adsorbed with the cerium precursor;
[0023] II. introducing an oxygen precursor into an atomic layer deposition device, and then performing a second chemical reaction to obtain a single-layer cerium oxide coating;
[0024] III. Repeat the operations of steps I and II to obtain a cerium oxide coating.
[0025] The present invention also provides the use of the composite coating described in the above technical solution or the composite coating prepared by the preparation method described in the above technical solution in an implant.
[0026] The present invention provides a composite coating, including an N-Cl type halamine coating, a copper-based nanozyme coating and a cerium oxide coating stacked from bottom to top. The cerium oxide particles in the cerium oxide coating in the composite coating provided by the present invention promote the osteogenic differentiation of bone marrow mesenchymal stem cells by producing platelet-derived growth factor-BB in a neutral environment, and block the internal copper-based nanozyme coating CuO NPs from contacting cells for a long time. After a large number of anaerobic bacteria adhere to the implant, the low-acid microenvironment formed locally destroys the cerium oxide, and the released CuO NPs can produce ROS (reactive oxygen) to play a bactericidal role. At the same time, the synergistic release of N-Cl in the N-Cl type halamine coating can enhance the oxidation activity of CuO NPs at low concentrations, thereby making the coating have excellent antibacterial properties without affecting the bone bonding of the implant. The experimental results show that the antibacterial rate of the composite coating provided by the present invention against Staphylococcus aureus is 94.6%, and the antibacterial rate against Escherichia coli is 94.48%; on the 7th and 14th days after cell inoculation on the surface of the sample, the expression of ALP in the composite coating is significantly higher than that of other samples. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 A schematic diagram of the principle of the composite coating provided by the present invention promoting osteogenesis in a neutral environment;
[0028] Figure 2 A schematic diagram of the antibacterial principle of the composite coating provided by the present invention in an acidic environment;
[0029] Figure 3 This is an electron microscope image of the composite coating prepared in Example 1;
[0030] Figure 4 The survival of the composite coating prepared in Example 1, the pure titanium sheet of Comparative Example 1, and the coatings prepared in Comparative Examples 2 to 3 on the agar plate after 12 hours of in vitro bacterial culture;
[0031] Figure 5The antibacterial rates of the composite coating prepared in Example 1, the pure titanium sheet in Comparative Example 1, and the coatings prepared in Comparative Examples 2 to 3 against Staphylococcus aureus;
[0032] Figure 6 The antibacterial rates of the composite coating prepared in Example 1, the pure titanium sheet in Comparative Example 1, and the coatings prepared in Comparative Examples 2 to 3 against Escherichia coli;
[0033] Figure 7 It is a statistical diagram of the antibacterial effect of the composite coating prepared in Example 1, the pure titanium sheet of Comparative Example 1, and the coatings prepared in Comparative Examples 2 to 3 after treatment;
[0034] Figure 8 The cell activities of the composite coating prepared in Example 1, the pure titanium sheet of Comparative Example 1, and the coatings prepared in Comparative Examples 2 to 3;
[0035] Fig. 9 The cell activities of the composite coating prepared in Example 1, the pure titanium sheet of Comparative Example 1, and the coatings prepared in Comparative Examples 2-3 after 7 and 14 days of culture. DETAILED DESCRIPTION
[0036] The invention provides a composite coating, comprising an N-Cl type halamine coating, a copper-based nanozyme coating and a cerium oxide coating which are sequentially stacked from bottom to top.
[0037] In the present invention, the composite coating includes an N-Cl type halamine coating. The release of N-Cl in the N-Cl type halamine coating can enhance the oxidation activity of CuO NPs at low concentrations, thereby making the coating have excellent antibacterial properties.
[0038] In the present invention, the thickness of the N-Cl type halamine coating is preferably 1-5 nm, more preferably 3 nm. When the thickness of the N-Cl type halamine coating is limited to the above range, the antibacterial performance of the coating can be further improved.
[0039] In the present invention, the composite coating further comprises a copper-based nanozyme coating disposed on the upper surface of the N-Cl type halamine coating. The copper-based nanozyme coating in the present invention can generate ROS (reactive oxygen species) to exert a bactericidal effect.
[0040] In the present invention, the thickness of the copper-based nanozyme coating is preferably 3 to 200 nm, more preferably 50 to 100 nm. When the thickness of the copper-based nanozyme coating is limited to the above range, the bactericidal performance can be further improved.
[0041] In the present invention, the composite coating further comprises a cerium oxide coating disposed on the upper surface of the copper-based nanozyme coating. The cerium oxide particles in the cerium oxide coating in the present invention promote the osteogenic differentiation of bone marrow mesenchymal stem cells by producing platelet-derived growth factor-BB in a neutral environment, and block the CuO NPs in the internal copper-based nanozyme coating from contacting cells for a long time, thereby not affecting the bone bonding of the implant.
[0042] In the present invention, the thickness of the cerium oxide coating is preferably 5 to 50 nm, more preferably 20 to 30 nm. The present invention limits the thickness of the cerium oxide coating to the above range, which can further promote the osteogenic differentiation of bone marrow mesenchymal stem cells.
[0043] The cerium oxide particles in the cerium oxide coating in the composite coating provided by the present invention promote the osteogenic differentiation of bone marrow mesenchymal stem cells by producing platelet-derived growth factor-BB in a neutral environment, and block the contact between CuO NPs in the internal copper-based nanozyme coating and cells for a long time. After a large number of anaerobic bacteria adhere to the implant, the low-acid microenvironment formed locally destroys the cerium oxide, and the released CuO NPs can produce ROS (reactive oxygen species) to exert a bactericidal effect. At the same time, the synergistic release of N-Cl in the N-Cl type halamine coating can enhance the oxidative activity of CuO NPs at low concentrations, thereby enabling the coating to have excellent antibacterial properties without affecting the bone integration of the implant.
[0044] The schematic diagram of the principle of the composite coating provided by the present invention promoting osteogenesis in a neutral environment is as follows Figure 1 shown.
[0045] from Figure 1 It can be seen that the cerium oxide particles in the composite coating provided by the present invention can promote the osteogenic differentiation of bone marrow mesenchymal stem cells.
[0046] The schematic diagram of the antibacterial principle of the composite coating provided by the present invention in an acidic environment is as follows Figure 2 shown.
[0047] from Figure 2 It can be seen that the composite coating provided by the present invention releases CuO NPs and generates ROS (reactive oxygen species) to exert a bactericidal effect. At the same time, the synergistic release of N-Cl in the N-Cl type halamine coating can enhance the oxidative activity of CuO NPs at low concentrations.
[0048] The present invention also provides a method for preparing the composite coating according to the above technical solution, which is characterized by comprising the following steps:
[0049] (1) preparing an N-Cl type halamine coating on the surface of a substrate;
[0050] (2) preparing a copper-based nanozyme coating by atomic layer deposition on the upper surface of the N-Cl type halamine coating obtained in step (1);
[0051] (3) A cerium oxide coating is prepared on the upper surface of the copper-based nanozyme coating obtained in step (2) by atomic layer deposition to obtain a composite coating.
[0052] The present invention has no particular limitation on the sources of the raw materials, and commercially available products known to those skilled in the art may be used.
[0053] The invention prepares an N-Cl type halogenamine coating on the surface of a substrate.
[0054] In the present invention, the substrate is preferably a titanium substrate. The present invention has no special limitation on the size of the titanium substrate, which can be adjusted according to actual needs.
[0055] In the present invention, the substrate is preferably pre-treated before use. The pre-treatment of the substrate in the present invention can remove impurities on the surface of the substrate.
[0056] In the present invention, the pretreatment preferably includes sanding, cleaning and drying performed in sequence.
[0057] In the present invention, the sandpaper polishing is preferably performed by using silicon carbide sandpaper. The present invention has no special limitation on the operation of the sandpaper polishing, and the oxide layer can be removed by using an operation well known to those skilled in the art.
[0058] In the present invention, the cleaning agents used for the cleaning are preferably acetone, ethanol and distilled water in sequence. The present invention has no special limitation on the specific cleaning operation, as long as the surface of the substrate is cleaned.
[0059] In the present invention, the drying is preferably air-drying. The present invention has no particular limitation on the air-drying operation, as long as the surface of the substrate is completely dried.
[0060] In the present invention, the preparation of the N-Cl type halamine coating on the substrate surface preferably comprises the following steps:
[0061] 1. Mixing a substrate with a halamine precursor solution and loading the substrate to obtain a substrate loaded with the halamine precursor;
[0062] 2. The substrate loaded with the halamine precursor obtained in step 1 is calcined to obtain an N-Cl type halamine coating.
[0063] In the present invention, the substrate is preferably mixed with a halamine precursor solution and loaded to obtain a substrate loaded with the halamine precursor.
[0064] In the present invention, the halamine precursor solution is preferably prepared by mixing a halamine precursor, ethanol and an acidic solution.
[0065] In the present invention, the halamine precursor is preferably ammonium chloride.
[0066] The present invention has no particular limitation on the amount of ethanol used, as long as the halamine precursor can be dissolved.
[0067] In the present invention, the acidic solution is preferably prepared from glacial acetic acid and distilled water. In the present invention, the volume ratio of the glacial acetic acid to distilled water is preferably 10:(1-3); the volume ratio of the ethanol to the glacial acetic acid in the acidic solution is preferably (2-6):1, more preferably 2.8:1. In the present invention, the acidic solution is a buffer solution for maintaining the pH of the solution.
[0068] In the present invention, the ratio of the mass of the halamine precursor to the volume of glacial acetic acid is preferably 10 mg: (0.5-1.5) mL, more preferably 10 mg: 1 mL.
[0069] The present invention has no special limitation on the operation of mixing the substrate and the halamine precursor solution. The solution can be stirred until transparent using a technical solution for preparing a mixed material well known to those skilled in the art.
[0070] In the present invention, the loading is preferably carried out under static conditions; the loading temperature is preferably room temperature; the loading time is preferably 3 to 24 hours, more preferably 4 hours. The present invention can increase the loading amount of the halamine precursor by limiting the loading temperature and time within the above ranges.
[0071] After the loading is completed, the present invention preferably dries the loaded product to obtain a matrix loaded with the halamine precursor.
[0072] The present invention has no particular limitation on the drying operation, and drying to a constant weight may be performed using an operation well known to those skilled in the art.
[0073] After obtaining the substrate loaded with the halamine precursor, the present invention preferably calcines the substrate loaded with the halamine precursor to obtain an N-Cl type halamine coating.
[0074] In the present invention, the calcination temperature is preferably 300-600°C, more preferably 500°C; the calcination time is preferably 1-5h, more preferably 1h. The present invention can calcine the halamine precursor into N-Cl chloride by calcination.
[0075] After the calcination is completed, the present invention preferably performs post-treatment on the product obtained by calcination to obtain an N-Cl type halamine coating.
[0076] In the present invention, the post-treatment includes washing and drying in sequence. The present invention adopts post-treatment to remove impurities on the surface of N-Cl type halamine coating.
[0077] The present invention has no special limitation on the cleaning operation, as long as the impurities on the surface of the N-Cl type halamine coating are cleaned away.
[0078] The present invention has no particular limitation on the drying operation, and drying to a constant weight may be performed using an operation well known to those skilled in the art.
[0079] After obtaining the N-Cl type halamine coating, the present invention uses an atomic layer deposition method to prepare a copper-based nanozyme coating on the upper surface of the N-Cl type halamine coating.
[0080] In the present invention, the atomic layer deposition method is preferably performed in an atomic layer deposition device. The present invention has no particular limitation on the model of the atomic layer deposition device, and any instrument or device well known to those skilled in the art can be used.
[0081] In the present invention, the operation of preparing the copper-based nanozyme coating by atomic layer deposition preferably comprises the following steps:
[0082] 1) introducing a copper precursor into an atomic layer deposition device, and then performing a first surface chemical adsorption reaction to obtain an N-Cl type halamine coating adsorbed with the copper precursor;
[0083] 2) introducing an oxygen precursor into an atomic layer deposition device, and then performing a first oxidation reaction to obtain a single-layer copper-based nanozyme coating;
[0084] 3) Repeat the operations of steps 1) and 2) to obtain a copper-based nanozyme coating.
[0085] The present invention preferably introduces a copper precursor into an atomic layer deposition device, and then performs a first surface chemical adsorption reaction to obtain an N-Cl type halamine coating adsorbed with the copper precursor.
[0086] In the present invention, nitrogen is preferably introduced into the atomic layer deposition device before the copper precursor is introduced into the atomic layer deposition device. In the present invention, nitrogen is introduced into the atomic layer deposition device before the copper precursor is introduced, so that air in the atomic layer deposition device can be removed.
[0087] In the present invention, the flow rate of the nitrogen is preferably 30 to 200 sccm, more preferably 50 sccm. The present invention has no particular limitation on the purity of the nitrogen, and nitrogen well known to those skilled in the art can be used. The present invention has no particular limitation on the time for introducing the nitrogen, as long as the air in the atomic layer deposition equipment is completely removed.
[0088] In the present invention, the copper precursor is preferably 1,1,1,5,5,5-hexafluoro-2,4-pentadicupper (3,3-dimethyl-1-butene)-copper (I). In the present invention, the copper precursor (hfac)Cu(DMB) is used to provide copper atoms for forming copper oxide.
[0089] In the present invention, the copper precursor is preferably introduced through a carrier gas; the carrier gas is preferably nitrogen; the flow rate of the carrier gas is preferably 30 to 200 sccm, more preferably 50 sccm.
[0090] In the present invention, the time for introducing the copper precursor is preferably 1 to 5 seconds, more preferably 1 to 2 seconds; the temperature of the copper precursor is preferably 30 to 50° C., more preferably 40° C. In the present invention, the time for introducing the copper precursor is the pulse time.
[0091] In the present invention, the time of the first surface chemical adsorption reaction is preferably 10 to 35 seconds, more preferably 18 to 25 seconds; the temperature of the first surface chemical adsorption reaction is preferably 80 to 120° C., more preferably 100° C. The present invention limits the temperature and time of the first surface chemical adsorption reaction to the above ranges so that chemical adsorption can occur on the substrate surface; in the present invention, the time of the first surface chemical adsorption reaction is the exposure time of the copper precursor.
[0092] After the first surface chemical adsorption reaction is completed, the present invention preferably purges the atomic layer deposition device to obtain an N-Cl type halamine coating adsorbed with a copper precursor. After the first surface chemical adsorption reaction is completed, the present invention purges the atomic layer deposition device to remove unreacted precursors in the device.
[0093] In the present invention, the gas used for the purge is preferably an inert gas, more preferably argon; the purge time is preferably 10 to 60 seconds, more preferably 15 seconds.
[0094] After obtaining the N-Cl type halamine coating adsorbed with the copper precursor, the present invention preferably introduces an oxygen precursor into the atomic layer deposition equipment, and then performs a first oxidation reaction to obtain a single-layer copper-based nanozyme coating.
[0095] In the present invention, the oxygen precursor is preferably ozone. In the present invention, the oxygen precursor is used to provide oxygen atoms.
[0096] In the present invention, the oxygen precursor is preferably introduced via a carrier gas; the carrier gas is preferably nitrogen; the flow rate of the carrier gas is preferably 30 to 200 sccm, more preferably 50 sccm.
[0097] In the present invention, the time for introducing the oxygen precursor is preferably 1 to 3 seconds, more preferably 1 second. In the present invention, the time for introducing the oxygen precursor is the pulse time of the oxygen precursor.
[0098] In the present invention, the time of the first oxidation reaction is preferably 5 to 30 seconds, more preferably 10 to 20 seconds; the temperature of the first oxidation reaction is preferably 80 to 120° C., more preferably 100° C. The present invention limits the temperature and time of the first oxidation reaction to the above ranges to produce copper oxide on the surface of the substrate; the time of the first oxidation reaction in the present invention is the exposure time of the oxygen precursor.
[0099] After the first oxidation reaction is completed, the present invention preferably purges the atomic layer deposition device to obtain a single-layer copper-based nanozyme coating. After the first oxidation reaction is completed, the present invention purges the atomic layer deposition device to remove unreacted precursors in the device.
[0100] In the present invention, the gas used for the purge is preferably an inert gas, more preferably argon; the purge time is preferably 10 to 60 seconds, more preferably 15 seconds.
[0101] After obtaining a single-layer copper-based nanozyme coating, the present invention preferably repeats the aforementioned operation of preparing a single-layer copper-based nanozyme coating to obtain a copper-based nanozyme coating. In the present invention, the single-layer copper-based nanozyme coating is a deposition cycle, and a copper-based nanozyme coating of a desired thickness can be prepared by repeatedly preparing a single-layer copper-based nanozyme coating.
[0102] The present invention has no particular limitation on the number of repetitions, which can be adjusted according to the desired thickness of the copper-based nanozyme coating.
[0103] After repeating the above-mentioned operation of preparing a single-layer copper-based nanozyme coating, the present invention preferably anneals the product obtained by repeating the above-mentioned operation of preparing a single-layer copper-based nanozyme coating to obtain a copper-based nanozyme coating. Annealing in the present invention can increase the binding sites of the copper-based nanozyme and improve the binding rate between the two coatings.
[0104] In the present invention, the annealing holding temperature is preferably 300-600° C., more preferably 350° C.; the annealing holding time is preferably 20-40 min, more preferably 30 min.
[0105] A copper-based nanozyme coating is obtained. The present invention uses an atomic layer deposition method to prepare a cerium oxide coating on the upper surface of the copper-based nanozyme coating to obtain a composite coating.
[0106] In the present invention, the atomic layer deposition method is preferably performed in an atomic layer deposition device. The present invention has no particular limitation on the model of the atomic layer deposition device, and any instrument or device well known to those skilled in the art can be used.
[0107] In the present invention, the operation of preparing the cerium oxide coating by the atomic layer deposition method comprises the following steps:
[0108] I. introducing a cerium precursor into an atomic layer deposition device, and then performing a second surface chemical adsorption reaction to obtain a copper-based nanozyme coating adsorbed with the cerium precursor;
[0109] II. introducing an oxygen precursor into an atomic layer deposition device, and then performing a second chemical reaction to obtain a single-layer cerium oxide coating;
[0110] III. Repeat the operations of steps I and II to obtain a cerium oxide coating.
[0111] The present invention preferably introduces a cerium precursor into an atomic layer deposition device, and then performs a second surface chemical adsorption reaction to obtain a copper-based nanozyme coating adsorbed with the cerium precursor.
[0112] In the present invention, nitrogen is preferably introduced into the atomic layer deposition device before the cerium precursor is introduced into the atomic layer deposition device. In the present invention, nitrogen is introduced into the atomic layer deposition device before the cerium precursor is introduced, so that air in the atomic layer deposition device can be removed.
[0113] In the present invention, the flow rate of the nitrogen is preferably 30 to 200 sccm, more preferably 50 sccm. The present invention has no particular limitation on the purity of the nitrogen, and nitrogen well known to those skilled in the art can be used. The present invention has no particular limitation on the time for introducing the nitrogen, as long as the air in the atomic layer deposition equipment is completely removed.
[0114] In the present invention, the cerium precursor is preferably Ce(iPrCp)3 or CE(TMHD)4 (tetrakis(2,2,6,6-tetramethyl-3,5-heptanedione)cerium(IV)). In the present invention, the cerium precursor is used to provide cerium atoms.
[0115] In the present invention, the cerium precursor is preferably introduced through a carrier gas; the carrier gas is preferably nitrogen; the flow rate of the carrier gas is preferably 30 to 200 sccm, more preferably 50 sccm.
[0116] In the present invention, the time for introducing the cerium precursor is preferably 0.2 to 3 seconds, more preferably 0.5 to 2 seconds; the temperature of the cerium precursor is preferably 140 to 160° C., more preferably 150° C. In the present invention, the time for introducing the cerium precursor is the pulse time of the cerium precursor.
[0117] In the present invention, the time of the second surface chemical adsorption reaction is preferably 10 to 30 seconds, more preferably 18 seconds; the temperature of the second surface chemical adsorption reaction is preferably 150 to 200° C., more preferably 200° C. The present invention limits the temperature and time of the second surface chemical adsorption reaction to the above ranges so that chemical adsorption can occur on the substrate surface; the time of the second surface chemical adsorption reaction in the present invention is the exposure time of the cerium precursor.
[0118] After the second surface chemical adsorption reaction is completed, the present invention preferably purges the atomic layer deposition device to obtain a copper-based nanozyme coating adsorbed with a cerium precursor. After the second surface chemical adsorption reaction is completed, the present invention purges the atomic layer deposition device to remove unreacted precursors in the device.
[0119] In the present invention, the gas used for the purge is preferably nitrogen; the purge time is preferably 10 to 30 seconds, more preferably 15 seconds.
[0120] After obtaining the copper-based nanozyme coating adsorbed with the cerium precursor, the present invention preferably introduces an oxygen precursor into the atomic layer deposition equipment, and then performs a second chemical reaction to obtain a single-layer cerium oxide coating.
[0121] In the present invention, the oxygen precursor is preferably deionized water. In the present invention, the oxygen precursor is used to provide oxygen atoms.
[0122] In the present invention, the oxygen precursor is preferably introduced via a carrier gas; the carrier gas is preferably nitrogen; the flow rate of the carrier gas is preferably 30 to 200 sccm, more preferably 50 sccm.
[0123] In the present invention, the time for introducing the oxygen precursor is preferably 0.1 to 2 seconds, more preferably 0.1 seconds. In the present invention, the time for introducing the oxygen precursor is the pulse time of the oxygen precursor.
[0124] In the present invention, the time of the second oxidation reaction is preferably 8 to 30 seconds, more preferably 10 to 12 seconds; the temperature of the second oxidation reaction is preferably 150 to 200° C., more preferably 200° C. The present invention limits the temperature and time of the first oxidation reaction to the above ranges to produce cerium oxide on the substrate surface; the time of the second oxidation reaction is the exposure time of the oxygen precursor.
[0125] After the second oxidation reaction is completed, the present invention preferably purges the atomic layer deposition device to obtain a single-layer cerium oxide coating. After the second oxidation reaction is completed, the present invention purges the atomic layer deposition device to remove unreacted precursors in the device.
[0126] In the present invention, the gas used for the purge is preferably nitrogen; the purge time is preferably 10 to 30 seconds, more preferably 15 seconds.
[0127] After obtaining the single-layer cerium oxide coating, the present invention preferably repeats the above-mentioned operation of preparing the single-layer cerium oxide coating to obtain the cerium oxide coating. The single-layer cerium oxide coating in the present invention is a deposition cycle, and the cerium oxide coating of the desired thickness can be prepared by repeating the operation of preparing the single-layer cerium oxide coating.
[0128] The present invention has no particular limitation on the number of repetitions, which can be adjusted according to the desired thickness of the cerium oxide coating.
[0129] In the present invention, the cerium oxide coating is preferably prepared at 0-1 Torr.
[0130] After obtaining the cerium oxide coating, the present invention preferably sequentially cleans and dries the cerium oxide coating to obtain a composite coating.
[0131] The present invention has no special limitation on the cleaning operation, as long as the surface of the cerium oxide coating is cleaned.
[0132] The present invention has no particular limitation on the drying operation, and the drying operation may be performed until the weight is constant.
[0133] The present invention can prepare a composite structure into a nano-layered film with high conformality, uniform texture, better hydrophilicity, antibacterial properties and corrosion resistance by continuously optimizing the atomic layer deposition conditions.
[0134] The present invention also provides the use of the composite coating described in the above technical solution or the composite coating prepared by the preparation method described in the above technical solution in an implant.
[0135] The present invention has no special limitation on the application operation of the composite coating in the implant, and the application operation well known to those skilled in the art can be adopted.
[0136] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0137] Example 1
[0138] The composite coating is composed of an N-Cl type halamine coating, a copper-based nanozyme coating and a cerium oxide coating which are stacked in sequence from bottom to top; wherein the thickness of the N-Cl type halamine coating is 3 nm, the thickness of the copper-based nanozyme coating is 50 nm, and the thickness of the cerium oxide coating is 20 nm;
[0139] The preparation method of the composite coating comprises the following steps:
[0140] (1) A titanium disc with a diameter of 9.5 mm and a thickness of 0.3 mm was polished step by step with different silicon carbide sandpapers ranging from 400# to 1500#, ultrasonically cleaned with acetone, ethanol and distilled water for 15 min respectively, and then air-dried to obtain a pretreated substrate;
[0141] (2) dissolving 100 mg of ammonium chloride in 28 mL of ethanol, adding 3 mL of distilled water and 10 mL of glacial acetic acid, placing the pretreated substrate obtained in step (1) in the above solution, stirring continuously until the solution is transparent, and then standing at room temperature for 4 hours, and then drying at 100° C. to obtain a substrate loaded with a halamine precursor;
[0142] (3) placing the substrate loaded with the halamine precursor obtained in step (2) in a muffle furnace and calcining it at 500° C. for 1 hour, then ultrasonically cleaning it with ethanol and distilled water for 15 minutes respectively, and then air-drying it to obtain an N-Cl type halamine coating;
[0143] (4) Preparation of a copper-based nanozyme coating on an atomic layer deposition device, the steps are as follows:
[0144] 1) introducing 50 sccm nitrogen into an atomic layer deposition device to remove air, then introducing (hfac)Cu(I)(DMB) for 1 second through 50 sccm carrier nitrogen, then performing a first surface chemical adsorption reaction at 100° C. for 18 seconds, and purging with argon for 15 seconds to obtain an N-Cl type halamine coating adsorbed with a copper precursor; wherein the temperature of the (hfac)Cu(I)(DMB) raw material bottle is maintained at 40° C. by heating with a heating jacket;
[0145] 2) In an atomic layer deposition device, ozone is introduced through 50 sccm of nitrogen as a carrier gas for 1 second, and then a first oxidation reaction is carried out at 100° C. for 10 seconds, followed by argon purge for 15 seconds to obtain a single-layer copper-based nanozyme coating; wherein the ozone is prepared by an ozone generator;
[0146] 3) Repeating the operations of steps 1) and 2), and then annealing at 350° C. for 30 min to obtain a copper-based nanozyme coating;
[0147] (5) Preparing a cerium oxide coating on an atomic layer deposition device, the steps are as follows:
[0148] I. Into the atomic layer deposition equipment, 50 sccm nitrogen was introduced to remove air, and then Ce(iPrCp)3 was introduced through 50 sccm carrier nitrogen for 0.5 s, and then a second surface chemical adsorption reaction was carried out at 200°C for 18 s, and then 50 sccm nitrogen was introduced for 15 s to obtain a copper-based nanozyme coating adsorbed with a cerium precursor; wherein the temperature of Ce(iPrCp)3 was maintained at 150°C;
[0149] II. In an atomic layer deposition device, deionized water was introduced through 50 sccm of nitrogen as a carrier gas for 0.1 s, and then a second oxidation reaction was carried out at 200° C. for 12 s, followed by 50 sccm of nitrogen purge for 15 s to obtain a single-layer cerium oxide coating; wherein the temperature of the deionized water raw material bottle was maintained at room temperature;
[0150] III. Repeat the operations of steps I and II to obtain a cerium oxide coating;
[0151] (6) The cerium oxide coating obtained in step (5) was ultrasonically cleaned with ethanol and distilled water for 15 minutes respectively, and vacuum-dried to obtain a composite coating, which was recorded as CeO2 / CuO NP / N-Cl composite coating (or CuONP / N-Cl composite coating).
[0152] The composite coating prepared in Example 1 was observed by field emission scanning electron microscopy. Figure 3 shown.
[0153] from Figure 3 It can be seen that the entire structure of the composite coating is smooth and complete.
[0154] Example 2
[0155] The composite coating is composed of an N-Cl type halamine coating, a copper-based nanozyme coating and a cerium oxide coating which are stacked in sequence from bottom to top; wherein the thickness of the N-Cl type halamine coating is 3 nm, the thickness of the copper-based nanozyme coating is 100 nm, and the thickness of the cerium oxide coating is 10 nm;
[0156] The preparation method of the composite coating comprises the following steps:
[0157] (1) A titanium disc with a diameter of 9.5 mm and a thickness of 0.3 mm was polished step by step with different silicon carbide sandpapers ranging from 400# to 1500#, ultrasonically cleaned with acetone, ethanol and distilled water for 15 min respectively, and then air-dried to obtain a pretreated substrate;
[0158] (2) dissolving 100 mg of ammonium chloride in 28 mL of ethanol, adding 3 mL of distilled water and 10 mL of glacial acetic acid, placing the pretreated substrate obtained in step (1) in the above solution, stirring continuously until the solution is transparent, and then standing at room temperature for 4 hours, and then drying at 100° C. to obtain a substrate loaded with a halamine precursor;
[0159] (3) placing the substrate loaded with the halamine precursor obtained in step (2) in a muffle furnace and calcining it at 500° C. for 1 hour, then ultrasonically cleaning it with ethanol and distilled water for 15 minutes respectively, and then air-drying it to obtain an N-Cl type halamine coating;
[0160] (4) Preparation of a copper-based nanozyme coating on an atomic layer deposition device, the steps are as follows:
[0161] 1) introducing 50 sccm nitrogen into an atomic layer deposition device to remove air, then introducing (hfac)Cu(I)(DMB) for 2 seconds through 50 sccm carrier nitrogen, then performing a first surface chemical adsorption reaction at 100° C. for 25 seconds, and purging with argon for 15 seconds to obtain an N-Cl type halamine coating adsorbed with a copper precursor; wherein the temperature of the (hfac)Cu(I)(DMB) raw material bottle is maintained at 40° C. by heating with a heating jacket;
[0162] 2) In an atomic layer deposition device, ozone is introduced through 50 sccm of nitrogen as a carrier gas for 1 second, and then a first oxidation reaction is carried out at 100° C. for 20 seconds, followed by argon purge for 15 seconds to obtain a single-layer copper-based nanozyme coating; wherein the ozone is prepared by an ozone generator;
[0163] 3) Repeating the operations of steps 1) and 2), and then annealing at 350° C. for 30 min to obtain a copper-based nanozyme coating;
[0164] (5) Preparing a cerium oxide coating on an atomic layer deposition device, the steps are as follows:
[0165] I. Into the atomic layer deposition equipment, 50 sccm nitrogen was introduced to remove air, and then Ce(iPrCp)3 was introduced through 50 sccm carrier gas nitrogen for 0.2 s, and then a second surface chemical adsorption reaction was carried out at 200°C for 10 s, and then 50 sccm nitrogen was introduced for 15 s to obtain a copper-based nanozyme coating adsorbed with a cerium precursor; wherein the temperature of Ce(iPrCp)3 was maintained at 150°C;
[0166] II. In an atomic layer deposition device, deionized water was introduced through 50 sccm of nitrogen as a carrier gas for 0.1 s, and then a second oxidation reaction was carried out at 200° C. for 10 s, followed by 50 sccm of nitrogen purge for 15 s to obtain a single-layer cerium oxide coating; wherein the temperature of the deionized water raw material bottle was maintained at room temperature;
[0167] III. Repeat the operations of steps I and II to obtain a cerium oxide coating;
[0168] (6) The cerium oxide coating obtained in step (5) is ultrasonically cleaned with ethanol and distilled water for 15 minutes respectively, and then air-dried in a vacuum to obtain a composite coating.
[0169] Example 3
[0170] The composite coating is composed of an N-Cl type halamine coating, a copper-based nanozyme coating and a cerium oxide coating which are stacked in sequence from bottom to top; wherein the thickness of the N-Cl type halamine coating is 3 nm, the thickness of the copper-based nanozyme coating is 200 nm, and the thickness of the cerium oxide coating is 50 nm;
[0171] The preparation method of the composite coating comprises the following steps:
[0172] (1) A titanium disc with a diameter of 9.5 mm and a thickness of 0.3 mm was polished step by step with different silicon carbide sandpapers ranging from 400# to 1500#, ultrasonically cleaned with acetone, ethanol and distilled water for 15 min respectively, and then air-dried to obtain a pretreated substrate;
[0173] (2) dissolving 100 mg of ammonium chloride in 28 mL of ethanol, adding 3 mL of distilled water and 10 mL of glacial acetic acid, placing the pretreated substrate obtained in step (1) in the above solution, stirring continuously until the solution is transparent, and then standing at room temperature for 4 hours, and then drying at 100° C. to obtain a substrate loaded with a halamine precursor;
[0174] (3) placing the substrate loaded with the halamine precursor obtained in step (2) in a muffle furnace and calcining it at 500° C. for 1 hour, then ultrasonically cleaning it with ethanol and distilled water for 15 minutes respectively, and then air-drying it to obtain an N-Cl type halamine coating;
[0175] (4) Preparation of a copper-based nanozyme coating on an atomic layer deposition device, the steps are as follows:
[0176] 1) introducing 50 sccm nitrogen into an atomic layer deposition device to remove air, then introducing (hfac)Cu(I)(DMB) through 50 sccm carrier nitrogen for 5 seconds, then performing a first surface chemical adsorption reaction at 100° C. for 35 seconds, and purging with argon for 15 seconds to obtain an N-Cl type halamine coating adsorbed with a copper precursor; wherein the temperature of the (hfac)Cu(I)(DMB) raw material bottle is maintained at 40° C. by heating with a heating jacket;
[0177] 2) In an atomic layer deposition device, ozone is introduced through 50 sccm of nitrogen as a carrier gas for 1 second, and then a first oxidation reaction is carried out at 100° C. for 30 seconds, followed by argon purge for 15 seconds to obtain a single-layer copper-based nanozyme coating; wherein the ozone is prepared by an ozone generator;
[0178] 3) Repeating the operations of steps 1) and 2), and then annealing at 350° C. for 30 min to obtain a copper-based nanozyme coating;
[0179] (5) Preparing a cerium oxide coating on an atomic layer deposition device, the steps are as follows:
[0180] I. Into the atomic layer deposition equipment, 50 sccm nitrogen was introduced to remove air, and then Ce(iPrCp)3 was introduced through 50 sccm carrier nitrogen for 2 seconds, and then a second surface chemical adsorption reaction was carried out at 200°C for 30 seconds, and then 50 sccm nitrogen was introduced for 15 seconds to obtain a copper-based nanozyme coating adsorbed with a cerium precursor; wherein the temperature of Ce(iPrCp)3 was maintained at 150°C;
[0181] II. In an atomic layer deposition device, deionized water was introduced through 50 sccm of nitrogen as a carrier gas for 0.1 s, and then a second oxidation reaction was performed at 200° C. for 30 s, followed by 50 sccm of nitrogen purge for 15 s to obtain a single-layer cerium oxide coating; wherein the temperature of the deionized water raw material bottle was maintained at room temperature;
[0182] III. Repeat the operations of steps I and II to obtain a cerium oxide coating;
[0183] (6) The cerium oxide coating obtained in step (5) is ultrasonically cleaned with ethanol and distilled water for 15 minutes respectively, and then air-dried in a vacuum to obtain a composite coating.
[0184] Comparative Example 1
[0185] Pure titanium discs are denoted as pure Ti group.
[0186] Comparative Example 2
[0187] On the basis of Example 1, the N-Cl type halamine coating and the copper-based nanozyme coating are omitted, that is, only the titanium disc and the cerium oxide coating on its upper surface (referred to as CeO2 group) are provided, and other conditions remain unchanged.
[0188] Comparative Example 3
[0189] On the basis of Example 1, the N-Cl type halamine coating and the cerium oxide coating were omitted, that is, only the titanium disc and the copper-based nanozyme coating on its upper surface (referred to as the CuO group) were provided, and other conditions remained unchanged.
[0190] The in vitro antibacterial performance of the composite coating prepared in Example 1, the pure titanium sheet of Comparative Example 1, and the coatings of Comparative Examples 2 to 3 was studied, and the test method was as follows:
[0191] 1. Bacterial recovery and cultivation
[0192] (1) Take out the overnight culture of bacteria from the -80°C freezer (150 times / min) and culture them overnight.
[0193] (2) Use a sterile inoculating loop to dip the overnight culture solution into a line on the solid culture medium and culture in a 37°C incubator for 24 h.
[0194] (3) Use a sterile inoculation loop to pick a single colony with regular morphology from the solid culture medium, transfer it to the liquid culture medium, and culture it overnight in a 37°C constant temperature shaking incubator (150 times / min).
[0195] (4) Repeat step (3) once to activate the bacteria.
[0196] (5) After bacterial thawing, several tubes of bacteria can be frozen and placed in a -80°C refrigerator for long-term storage to prevent bacterial contamination during the experiment.
[0197] 2. In vitro antibacterial activity test
[0198] (1) Two common microorganisms, Staphylococcus aureus (S. aureus) and Escherichia coli (E. coli), were tested on the surface of each sterilized sample and cultured in liquid TSB and LB medium, respectively. After culturing overnight at 37°C, the bacterial suspension was diluted to 1-fold and cultured to 10 6 CFU / mL.
[0199] (2) 100 μL of bacterial suspension and 400 mL of LB or TSB medium were added to EP tubes at the same time, and cultured with the prepared samples at 37°C for 12 h.
[0200] (3) Take out 100 μL of the co-cultured bacterial suspension and perform gradient dilution. Finally, evenly spread 50 μL of the diluted bacterial suspension on the nutrient agar medium, culture at 37°C for 18 hours, and finally count the number of colonies. The experiment was repeated 3 times for each group, and the antibacterial effect was calculated as follows. Among them, Is is the number of colonies in the test sample, Ic is the total number of colonies in the control group, and the antibacterial rate (%) = Ic-Is / Ic×100%.
[0201] After in vitro bacterial culture for 12 hours, the survival rate of the composite coating prepared in Example 1, the pure titanium sheet of Comparative Example 1 and the coating prepared in Comparative Examples 2 to 3 on the agar plate is as follows: Figure 4 As shown; the antibacterial rate of the composite coating prepared in Example 1, the pure titanium sheet of Comparative Example 1 and the coating prepared in Comparative Examples 2 to 3 against Staphylococcus aureus is as shown Figure 5 As shown; the antibacterial rate of the composite coating prepared in Example 1, the pure titanium sheet of Comparative Example 1 and the coating prepared in Comparative Examples 2 to 3 against Escherichia coli is as follows Figure 6 As shown; * indicates p < 0.05, ** indicates p < 0.01.
[0202] from Figure 4 It can be seen that after adding CeO2 coating, CuO coating and composite coating to the Ti wafer in sequence, the number of bacterial colonies decreased significantly; the composite coating group had the least CFU, followed by the CeO2 group and the CuO group, and the pure titanium control group had the largest number of CFU.
[0203] from Figure 5 It can be seen that the antibacterial rate of the composite coating group against Staphylococcus aureus was 94.6%, which was significantly higher than that of the Ti, CeO2 and CuO groups (p<0.001).
[0204] from Figure 6 It can be seen that the antibacterial rate of the composite coating group against Escherichia coli was 94.48%, which was significantly higher than that of the Ti, CeO2 and CuO groups (p<0.001).
[0205] from Figures 4 to 6 It can be seen that the composite coating has a significant inhibitory effect on bacterial growth.
[0206] The micro-implant culture bacterial suspension was taken from the femoral specimen, plated and cultured, and then the colony count was performed. Figure 7 As shown, Figure 7 It is a statistical chart of the antibacterial effect of the composite coating prepared in Example 1, the pure titanium sheet of Comparative Example 1, and the coatings prepared in Comparative Examples 2 to 3 after treatment.
[0207] from Figure 7 It can be seen that the antibacterial rate of the composite coating group is as high as 98.26%, which is significantly higher than that of the Ti, CeO2 and CuO group samples (p<0.001).
[0208] Both in vivo and in vitro antibacterial experiments showed that the composite coating exhibited excellent potential in antibacterial properties.
[0209] The composite coating prepared in Example 1, the pure titanium sheet of Comparative Example 1, and the coatings of Comparative Examples 2 to 3 were tested for osteogenic performance. The test method is as follows:
[0210] (1) Place the sterilized sample into a 48-well plate.
[0211] (2) Use a micropipette to measure 500 μL of cells with a density of 3×10 4 Inoculate the MC3T3-E1 cell suspension of 100 μl / well into the sample in the well plate, and make sure that the cells are dispersed evenly by blowing to avoid clumping. Place the well plate in a cell culture incubator for culture.
[0212] (3) After 24 hours, discard the original cell culture medium, wash with PBS and replace with osteogenic induction culture medium. Continue to culture in the cell culture incubator for 7 days and 14 days respectively, and replace the cell culture medium after about 48 hours.
[0213] (4) Discard the original cell culture medium and rinse with PBS. Use a micropipette to measure 150 μL of RIPA (containing 1 mM PMSF) cell lysis solution and transfer it to each well. Shake the plate to allow the cell lysis solution to fully contact the cells. Place the plate on ice and lyse for 30 minutes.
[0214] (5) Pipette the lysate repeatedly and collect it into a 1.5 mL EP tube. Place it in a high-speed centrifuge precooled to 4°C. Centrifuge at a set speed of 12,000 r / min for 5 min.
[0215] (6) Take 25 μL of cell lysate and 200 μL of BCA working solution and add them to a 96-well plate. Gently shake to mix thoroughly and place in a 37°C incubator for 30 min. Detect the OD value with a microplate reader at a wavelength of 562 nm. Calculate the total cell protein concentration (gpro / mL) based on the BCA standard curve.
[0216] (7) Determine ALP activity according to the instructions of the ALP kit. After each well is fully mixed, place it at 37°C for 15 minutes, take out each well, add 150 μg of color developer and continue mixing. Measure the OD value with a microplate reader at a wavelength of 520 nm to calculate the ALP activity. Divide the ALP activity by the total cell protein concentration and normalize and calculate the relative ALP activity per gram of protein (king unit / gpro).
[0217] The cell activity of the composite coating prepared in Example 1, the pure titanium sheet of Comparative Example 1, and the coatings prepared in Comparative Examples 2 to 3 are shown in FIG. Figure 8 As shown; the cell activity of the composite coating prepared in Example 1, the pure titanium sheet of Comparative Example 1 and the coating prepared in Comparative Examples 2 to 3 after 7 days and 14 days of culture is shown in Fig. 9 As shown; * indicates p < 0.05, ** indicates p < 0.01.
[0218] from Figure 8 It can be seen that after 1 day, the cell viability on CeO2, CuO and composite coating group samples was significantly higher than that on pure Ti; as the culture time increased from 1 day to 7 days, the cell proliferation of the composite coating group samples increased significantly.
[0219] from Fig. 9 It can be seen that on the 7th and 14th days after cell inoculation on the sample surface, the expression level of ALP in the composite coating group was significantly higher than that in other samples.
[0220] It can be seen from the above embodiments that the composite coating provided by the present invention does not affect the bone integration of the implant and has excellent antibacterial properties.
[0221] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A composite coating, comprising an N-Cl type halamine coating, a copper-based nanozyme coating and a cerium oxide coating stacked in sequence from bottom to top.
2. The composite coating according to claim 1, characterized in that: The thickness of the N-Cl type halogenamine coating is 1 to 5 nm.
3. The composite coating according to claim 1, characterized in that: The thickness of the copper-based nanozyme coating is 3 to 200 nm.
4. The composite coating according to claim 1, characterized in that: The thickness of the cerium oxide coating is 5 to 50 nm.
5. The method for preparing the composite coating according to any one of claims 1 to 4, characterized in that: The steps include: (1) preparing an N-Cl type halamine coating on the surface of a substrate; (2) preparing a copper-based nanozyme coating on the upper surface of the N-Cl type halamine coating obtained in step (1) by atomic layer deposition; (3) A cerium oxide coating is prepared on the upper surface of the copper-based nanozyme coating obtained in step (2) by atomic layer deposition to obtain a composite coating.
6. The preparation method according to claim 5, characterized in that: The atomic layer deposition methods in step (2) and step (3) are independently performed in atomic layer deposition equipment.
7. The preparation method according to claim 6, characterized in that: The process of preparing the copper-based nanozyme coating by atomic layer deposition comprises the following steps: 1) introducing a copper precursor into an atomic layer deposition device, and then performing a first surface chemical adsorption reaction to obtain an N-Cl type halamine coating adsorbed with the copper precursor; 2) introducing an oxygen precursor into an atomic layer deposition device, and then performing a first oxidation reaction to obtain a single-layer copper-based nanozyme coating; 3) Repeat the operations of steps 1) and 2) to obtain a copper-based nanozyme coating.
8. The preparation method according to claim 7, characterized in that: The time for introducing the copper precursor in step 1) is 1 to 5 seconds.
9. The preparation method according to claim 6, characterized in that: The process of preparing the cerium oxide coating by atomic layer deposition comprises the following steps: I. introducing a cerium precursor into an atomic layer deposition device, and then performing a second surface chemical adsorption reaction to obtain a copper-based nanozyme coating adsorbed with the cerium precursor; II. introducing an oxygen precursor into an atomic layer deposition device, and then performing a second chemical reaction to obtain a single-layer cerium oxide coating; III. Repeat the operations of steps I and II to obtain a cerium oxide coating.
10. Use of the composite coating according to any one of claims 1 to 4 or the composite coating prepared by the preparation method according to any one of claims 5 to 9 in implants.