Preparation method of lithium manganese iron phosphate, positive electrode material and lithium ion battery

By using metal organic framework materials to prepare lithium manganese iron phosphate, the problems of poor conductivity and circulation performance of lithium manganese iron phosphate are solved, the conductivity and cycle life are improved, and the efficient lithium-ion battery material is formed.

CN119018869APending Publication Date: 2024-11-26PHYLION-QINGYUAN (SICHUAN) NEW MATERIAL TECH CO LTD +1

Patent Information

Application Number
CN202411085474.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The current lithium manganese phosphate has poor conductivity and cycle performance, resulting in poor conductivity and cycle life of the battery.

Method used

The metal organic framework materials in manganese sources and iron sources are prepared by sintering, and mixed with lithium sources, phosphorus sources and carbon sources to form lithium manganese phosphate. By controlling the sintering temperature and time, a porous structure is formed. Improve the diffusion and conductivity of lithium ions.

Benefits of technology

It significantly improves the conductivity and cycle life of lithium manganese iron phosphate, extends the cycle life of the battery, and improves the compaction density of the material and the first discharge specific capacity of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018869A_ABST
    Figure CN119018869A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium ion batteries, in particular to a preparation method of lithium iron manganese phosphate, a positive electrode material and a lithium ion battery, and at least one of a manganese source and an iron source is adopted as a metal organic framework material as a metal source to prepare a manganese iron oxide precursor for preparing lithium iron manganese phosphate. The metal organic framework material is a crystalline porous material formed by connecting metal ions and organic ligands through coordinate bonds, and after sintering is carried out under the condition of 300-1200 DEG C, the internal organic ligands are removed, so that a metal oxide with a nano-sized porous structure is formed; diffusion of lithium and diffusion of battery material lithium ions in the lithium mixed sintering process are facilitated, and the conductivity and the cycle performance of lithium manganese iron phosphate prepared by sintering at 500-900 DEG C are greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a method for preparing lithium manganese iron phosphate, a positive electrode material and a lithium ion battery. Background Art

[0002] In the field of new energy batteries, lithium manganese iron phosphate (LMFP) is widely used in electric vehicles, energy storage systems and other fields due to its advantages such as high energy density, long cycle life and environmental friendliness. However, the electrochemical properties of lithium manganese iron phosphate are affected by its precursor materials. Therefore, finding suitable precursor materials is the key to improving the performance of lithium manganese iron phosphate. Currently commonly used precursors include Mn3O4, Fe2O3, FePO4, etc. LMFP is prepared by grinding and mixing manganese source, iron source, phosphorus source, carbon source, etc. in a certain proportion and solid phase sintering. However, too many components mean that this requires more cost and a more efficient grinding process. Chinese patent CN115744861B discloses a lithium manganese iron phosphate precursor NH4Mn 1-x Fe x PO4 synthesis method, but the reduction ammonia gas is generated during the lithium sintering process, which will cause the product to produce Fe2P and other impurities; Chinese patent CN117125690A discloses a method of using ferromanganese pyrophosphate as a precursor for the synthesis of lithium iron manganese phosphate, but the prepared precursor is a flaky morphology, resulting in low material compaction; the generation of impurities or low compaction density will lead to poor conductivity and cycle performance of the battery. Summary of the invention

[0003] Therefore, the technical problem to be solved by the present invention is to overcome the defects of poor conductivity and cycle performance of lithium manganese iron phosphate synthesized in the prior art, thereby providing a preparation method of lithium manganese iron phosphate, a positive electrode material and a lithium ion battery.

[0004] To this end, the present invention provides a method for preparing lithium manganese iron phosphate, comprising the following steps:

[0005] Step S1: mixing a manganese source and an iron source to obtain a first mixture; at least one of the manganese source and the iron source is a metal organic framework material;

[0006] Step S2: sintering the first mixture at 300-1200° C. to obtain ferromanganese oxide;

[0007] Step S3: mixing the manganese iron oxide with the lithium source, the phosphorus source and the carbon source and drying the mixture to obtain a second mixture;

[0008] Step S4: sintering the second mixture at 500-900° C. to obtain lithium manganese iron phosphate.

[0009] Furthermore, the manganese source is one or more of manganese-based metal-organic framework materials, elemental manganese, manganese tetraoxide, manganese trioxide, manganous oxide, manganese oxide, manganese dioxide, monohydroxy manganese oxide MnO(OH), hydrated manganese dioxide MnO(OH)2, manganese hydroxide Mn(OH)2, manganese carbonate, manganese sulfate, manganese nitrate, manganese citrate, manganese oxalate, manganese formate, manganese acetate, and manganese phosphate.

[0010] Furthermore, the manganese-based metal organic framework material is composed of a manganese salt and an organic ligand connected by a coordination bond. The present invention does not limit the manganese salt, organic ligand and synthesis method required for the synthesis.

[0011] In certain preferred embodiments, in order to further improve the electrical properties of lithium manganese iron phosphate, the manganese salt is MnCl2·4H2O, and the organic ligand is 2,5-dihydroxyterephthalic acid.

[0012] Further, the iron source is one or more of iron-based metal-organic framework materials, elemental iron, ferroferric oxide, ferrous oxide, basic iron oxide FeO(OH), ferric hydroxide, ferrous hydroxide, ferrous sulfate, ferric sulfate, ferric nitrate, ferric nitrate nonahydrate, ferrous nitrate, ferrous chloride, ferric bromide, ferric phosphate, ferrous phosphate, ferrous carbonate, ferric oxalate, ferrous oxalate, ferrous acetate, ferric citrate, and ferrous citrate.

[0013] Furthermore, the iron-based metal organic framework material is composed of an iron salt and an organic ligand connected by a coordination bond. The present invention does not limit the iron salt, organic ligand and synthesis method required for synthesis.

[0014] In certain preferred embodiments, in order to further improve the electrical properties of lithium manganese iron phosphate, the iron salt is FeCl3·6H2O and the organic ligand is terephthalic acid.

[0015] Furthermore, in step S1, the molar ratio of the iron element in the iron source to the manganese element in the manganese source is 1:9-9:1, preferably 4:6.

[0016] In certain preferred embodiments, in order to further improve the conductivity and cycle performance of lithium manganese iron phosphate, the sintering temperature in step S1 is 550-650° C. and the sintering time is 4.5-5.5 hours.

[0017] In certain preferred embodiments, in order to further improve the conductivity and cycle performance of lithium manganese iron phosphate, the sintering temperature of step S2 is 650-750° C. and the sintering time is 7.5-8.5 hours.

[0018] Furthermore, in step S3, compounds containing other elements may be added, preferably, the other elements are at least one of Al, Cr, Co, Fe, Mg, Ti, V, Ni, Cu, Zn, Zr, Nb, Mo, W, Ca, Y, La, Ce, Ga, and In. The compound containing other elements is at least one of oxides containing other elements, hydroxides containing other elements, halides containing other elements, sulfates containing other elements, carbonates containing other elements, nitrates containing other elements, and oxynitrates containing other elements.

[0019] Furthermore, the molecular formula of the lithium iron manganese phosphate is: LiMn x Fe 1-x PO4, wherein 0<x<1; and / or, the lithium source is one or more of lithium carbonate, lithium hydroxide, lithium oxide, lithium peroxide, lithium bicarbonate, lithium phosphate, lithium dihydrogen phosphate, dilithium hydrogen phosphate, lithium oxalate, lithium acetate, lithium sulfate, lithium nitrate, lithium chloride, lithium sulfide, lithium citrate, lithium benzoate, lithium borate, lithium metaborate, and lithium tetrachloroborate; and / or, the phosphorus source is one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium tripolyphosphate, phosphoric acid, calcium phosphate, phosphate ester, lithium dihydrogen phosphate, iron phosphate, lithium phosphate, lithium dihydrogen phosphate, and manganese phosphate.

[0020] Furthermore, the carbon source is one or more of glucose, citric acid, urea, melamine, sodium gluconate, sodium citrate, polyethylene glycol, soybean meal, fructose, starch, phenolic resin, and vitamin C; and / or the ratio of the molar amount of the carbon source to the molar amount of the lithium source is 1:5-1:50.

[0021] Furthermore, the drying is spray drying.

[0022] The present invention also provides a positive electrode material, comprising lithium manganese iron phosphate prepared by any of the above preparation methods.

[0023] The present invention also provides a lithium ion battery, comprising a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator, wherein the positive electrode sheet is made of the positive electrode material described above.

[0024] The technical solution of the present invention has the following advantages:

[0025] 1. The method for preparing lithium manganese iron phosphate provided by the present invention comprises the following steps: step S1: mixing a manganese source and an iron source to obtain a first mixture; at least one of the manganese source and the iron source is a metal organic framework material; step S2: sintering the first mixture at 300 to 1200° C. to obtain manganese iron oxide; step S3: mixing the manganese iron oxide with a lithium source, a phosphorus source and a carbon source and drying them to obtain a second mixture; step S4: sintering the second mixture at 500 to 900° C. to obtain lithium manganese iron phosphate. The present invention uses at least one of the manganese source and the iron source as a metal organic framework material as a metal source to prepare a manganese iron oxide precursor for preparing lithium manganese iron phosphate. The metal-organic framework material is a crystalline porous material composed of metal ions and organic ligands connected by coordination bonds. After sintering at 300-1200°C, the internal organic ligands are removed to form a metal oxide with a nano-sized porous structure, which is beneficial to the diffusion of lithium and the diffusion of lithium ions in the battery material during the mixed lithium sintering process. The conductivity and cycle performance of lithium iron manganese phosphate sintered at 500-900°C are greatly improved, and the cycle life is significantly extended.

[0026] 2. The preparation method of lithium manganese iron phosphate provided by the present invention, in a preferred embodiment, by using MnCl2·4H2O as a manganese salt and 2,5-dihydroxyterephthalic acid as an organic ligand to prepare a manganese-based metal organic framework material MOF-74 (Mn), the manganese-based metal organic framework material has a high specific surface area, rich microporous structure, and has open metal nodes and oxygen-rich dicarboxylic acid ligands (O% = 48.5%), and is an ideal template for preparing hybrid materials. The conductivity and cycle life of lithium manganese iron phosphate prepared by the method of the present invention using it as a raw material are further improved.

[0027] 3. The preparation method of lithium manganese iron phosphate provided by the present invention, in a preferred embodiment, by using FeCl3·6H2O as the iron salt and terephthalic acid as the organic ligand to prepare the iron-based metal organic framework material MIL-101 (Fe), which has the advantages of flexible structure, large specific surface area, large porosity, adjustable pore size, etc., and the conductivity and cycle life of the lithium manganese iron phosphate prepared by the method of the present invention using it as the raw material are further improved.

[0028] 4. The preparation method of lithium manganese iron phosphate provided by the present invention has better conductivity by controlling the molar ratio of the iron element in the iron-based metal-organic framework material and the manganese element in the manganese-based metal-organic framework material to be 1:9-9:1, especially 4:6. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0030] Figure 1 is a SEM image of the manganese iron oxide prepared in Example 1;

[0031] Figure 2 is a SEM image of lithium manganese iron phosphate prepared in Example 1;

[0032] Figure 3 is the discharge curve of the lithium ion battery obtained from the lithium manganese iron phosphate of Example 1;

[0033] Figure 4 This is the discharge curve of the lithium-ion battery obtained from the lithium manganese iron phosphate in Comparative Example 1. DETAILED DESCRIPTION

[0034] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0035] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0036] Among them, the preparation method of Mn-MOF in the following embodiments and comparative examples is as follows: the manganese source is MnCl2·4H2O, the organic ligand is 2,5-dihydroxyterephthalic acid, 1.187g of manganese source is dissolved in 6mL of ethanol and water mixed solution (the volume ratio of ethanol and water in the mixed solution is 1:1) to obtain a manganese-containing solution. 0.396g of organic ligand is dissolved in 45mL of N,N-dimethylformamide (DMF) solution to obtain an organic ligand solution. The organic ligand solution is poured into the above-mentioned manganese-containing solution, stirred at room temperature for 30 minutes, and then placed in a polytetrafluoroethylene-lined hydrothermal autoclave, and kept at 135°C for 24h to obtain a metal organic framework material MOF-74 (Mn), which is then washed and dried to obtain a dry product, recorded as Mn-MOF.

[0037] The preparation method of Fe-MOF is as follows: the iron source is FeCl3·6H2O, and the organic ligand is terephthalic acid. 1.352g of the iron source and 0.422g of the organic ligand are dissolved in 30mL of N,N-dimethylformamide (DMF), then put into a polytetrafluoroethylene-lined hydrothermal autoclave, and kept at 110°C for 20h to obtain the metal organic framework material MIL-101 (Fe), which is then washed and dried to obtain a dry product, recorded as Fe-MOF.

[0038] Example 1

[0039] This embodiment provides a method for preparing lithium manganese iron phosphate, comprising the following steps:

[0040] Step S1: Mn-MOF and Fe-MOF are mixed at a molar ratio of manganese to iron of 6:4 to obtain a first mixture;

[0041] Step S2: placing the first mixture at 600°C in an air atmosphere for solid phase sintering for 5 hours to obtain manganese iron oxide Mn 0.6 Fe 0.4 O x ;

[0042] Step S3: Manganese iron oxide Mn 0.6 Fe 0.4 O x , lithium dihydrogen phosphate and glucose in a molar ratio of 1:1.05:0.1 and then spray-dried to obtain a second mixture;

[0043] Step S4: The second mixture is placed at 700°C in a nitrogen atmosphere for solid phase sintering for 8 hours to obtain lithium manganese iron phosphate, molecular formula: LiMn 0.6 Fe 0.4 PO4.

[0044] Among them, the SEM images of manganese iron oxide and lithium manganese iron phosphate are shown in Figure 1 and Figure 2 .

[0045] Example 2

[0046] This embodiment provides a method for preparing lithium manganese iron phosphate, which is basically the same as Example 1, except that Fe(NO3)3·9H2O is used instead of Fe-MOF in step S1, and Mn-MOF and Fe(NO3)3·9H2O are mixed at a molar ratio of manganese to iron elements of 6:4.

[0047] Example 3

[0048] This embodiment provides a method for preparing lithium manganese iron phosphate, which is basically the same as that of Embodiment 1, except that Mn3O4 is used instead of Fe-MOF in step S1, and Mn3O4 and Fe-MOF are mixed at a molar ratio of manganese to iron elements of 6:4.

[0049] Example 4

[0050] This embodiment provides a method for preparing lithium manganese iron phosphate, which is basically the same as that in Example 1, except that in step S1, Mn-MOF and Fe-MOF are mixed at a molar ratio of manganese and iron elements of 8:2, and the remaining process steps are the same as those in Example 1. The molecular formula of the lithium manganese iron phosphate finally prepared is: LiMn 0.8 Fe 0.2 PO4.

[0051] Example 5

[0052] This embodiment provides a method for preparing lithium manganese iron phosphate, which is basically the same as that in embodiment 1, except that in step S1, Mn-MOF and Fe-MOF are mixed at a molar ratio of manganese and iron elements of 2:8, and the remaining process steps are the same as those in embodiment 1. The molecular formula of the lithium manganese iron phosphate finally prepared is: LiMn 0.2 Fe 0.8 PO4.

[0053] Example 6

[0054] This embodiment provides a method for preparing lithium manganese iron phosphate, comprising the following steps:

[0055] Step S1: Mn-MOF and Fe-MOF are mixed at a molar ratio of manganese to iron of 6:4 to obtain a first mixture;

[0056] Step S2: The first mixture is placed in an air atmosphere at 650° C. for solid phase sintering for 5.5 hours to obtain manganese iron oxide Mn 0.6 Fe 0.4 O x ;

[0057] Step S3: Manganese iron oxide Mn 0.6 Fe 0.4 O x , lithium dihydrogen phosphate and glucose in a molar ratio of 1:1.05:0.1 and then spray-dried to obtain a second mixture;

[0058] Step S4: The second mixture is placed at 550°C in a nitrogen atmosphere for solid phase sintering for 8.5 hours to obtain lithium manganese iron phosphate, molecular formula: LiMn 0.6 Fe 0.4 PO4.

[0059] Example 7

[0060] This embodiment provides a method for preparing lithium manganese iron phosphate, comprising the following steps:

[0061] Step S1: Mn-MOF and Fe-MOF are mixed at a molar ratio of manganese to iron of 6:4 to obtain a first mixture;

[0062] Step S2: placing the first mixture at 550° C. in an air atmosphere for solid phase sintering for 5.5 hours to obtain manganese iron oxide Mn 0.6 Fe 0.4 O x ;

[0063] Step S3: Manganese iron oxide Mn 0.6 Fe 0.4 O x , lithium dihydrogen phosphate and glucose in a molar ratio of 1:1.05:0.1 and then spray-dried to obtain a second mixture;

[0064] Step S4: The second mixture is placed in a nitrogen atmosphere at 650°C for solid phase sintering for 7.5 hours to obtain lithium manganese iron phosphate, molecular formula: LiMn 0.6 Fe 0.4 PO4.

[0065] Example 8

[0066] This embodiment provides a method for preparing lithium manganese iron phosphate, which is basically the same as that of Embodiment 1, except that the sintering temperature of step S1 is 450° C., and the sintering temperature of step S2 is 900° C.

[0067] Example 9

[0068] This embodiment provides a method for preparing lithium manganese iron phosphate, which is basically the same as that of Embodiment 1, except that the sintering temperature of step S1 is 1200° C., and the sintering temperature of step S2 is 500° C.

[0069] Comparative Example 1

[0070] This comparative example provides a method for preparing lithium manganese iron phosphate, which is basically the same as Example 4, except that in step S1, Fe(NO3)3·9H2O is used instead of Fe-MOF, Mn3O4 is used instead of Fe-MOF, and Mn3O4 and Fe(NO3)3·9H2O are mixed in a molar ratio of manganese and iron elements of 6:4.

[0071] Comparative Example 2

[0072] This comparative example provides a method for preparing lithium manganese iron phosphate, comprising the following steps:

[0073] Step S1: Mn-MOF, Fe-MOF, lithium dihydrogen phosphate and glucose are mixed in a molar ratio of manganese iron lithium element to glucose of 0.8:0.2:1.05:0.1, and then spray-dried to obtain a first mixture;

[0074] Step S2: The first mixture is placed at 700°C in a nitrogen atmosphere for solid phase sintering for 6 hours to obtain lithium manganese iron phosphate, molecular formula: LiMn 0.8 Fe 0.2 PO4.

[0075] Comparative Example 3

[0076] This comparative example provides a method for preparing lithium manganese iron phosphate, comprising the following steps:

[0077] Step S1: Mn-MOF, Fe-MOF, lithium dihydrogen phosphate and glucose are mixed in a molar ratio of lithium manganese iron element to glucose of 0.2:0.8:1.05:0.1, and then spray-dried to obtain a first mixture;

[0078] Step S2: The first mixture is placed in an air atmosphere at 600°C for solid phase sintering for 5 hours, and then in a nitrogen atmosphere at 700°C for solid phase sintering for 8 hours to obtain lithium manganese iron phosphate, molecular formula: LiMn 0.2 Fe 0.8 PO4.

[0079] Experimental Example 1

[0080] The compaction density of the lithium manganese iron phosphate obtained in each embodiment and comparative example was tested, as shown in Table 1.

[0081] The conductivity of the lithium manganese iron phosphate prepared in each embodiment and comparative example was tested. The test method was as follows: a four-probe tester was used for testing. The powder was placed on a tablet press and a pressure of 30 MPa was applied. After maintaining the pressure for 1 minute, the resistance was measured, the pressure was released, and finally the mold height was measured. The results are shown in Table 1.

[0082] Table 1 Conductivity and compaction density of lithium manganese iron phosphate in various embodiments and comparative examples

[0083]

[0084]

[0085] It can be seen from the above table that, compared with Comparative Examples 1-3, the conductivity of lithium manganese iron phosphate prepared in each embodiment of the present invention is significantly improved, especially in Embodiments 1, 6 and 7.

[0086] Compared with comparative examples 1-3, the compaction density of lithium iron manganese phosphate prepared in examples 1-7 and 9 of the present invention is significantly improved, especially examples 1, 3, 5 and 7.

[0087] Experimental Example 2

[0088] The cycle performance of the lithium ion battery made of lithium manganese iron phosphate prepared in each embodiment and comparative example was tested. The preparation method of the lithium ion battery is as follows: lithium manganese iron phosphate, conductive agent CNT and adhesive PVDF are mixed in a solvent (NMP) at a fixed mass ratio of 80:15:5, and evenly coated on the current collector aluminum foil after stirring, pressed and dried, and then cut into a disc with a diameter of 12mm to finally obtain the positive electrode of the button battery. A lithium sheet (thickness of 0.6mm) is used as the negative electrode, fluoroethylene carbonate, dimethyl carbonate and ethylene carbonate (volume ratio of 10:45:45) containing 1mol / L LiPF6 are used as the electrolyte, and the purchased polypropylene film is cut and used as a diaphragm, and the button battery is assembled in the argon atmosphere of the glove box.

[0089] The test method is as follows: the test voltage is set to 2.5-4.3V, and the test temperature is strictly maintained at 25°C. The battery test system (LAND CT2001A) is used to test the first discharge gram capacity of the button battery at 0.1C and the cycle performance at 1C, and the capacity retention rate after 200 cycles at 1C is calculated. The results are shown in Table 2.

[0090] Table 2 Discharge specific capacity and capacity retention rate results

[0091]

[0092] As can be seen from the above table, compared with Comparative Examples 1-3, the cycle performance of the lithium ion battery made of lithium manganese iron phosphate provided by each embodiment of the present invention is not only significantly improved, the cycle life is significantly extended, but also the first discharge specific capacity is significantly improved, especially in Examples 1, 6 and 7. Figure 3 and Figure 4 .

[0093] Comparing Example 1 with Examples 2-3, it can be seen that the cycle performance and first discharge specific capacity of the lithium-ion battery prepared by using metal organic framework materials as both the manganese source and the iron source in Example 1 are further improved.

[0094] Comparing Example 1 with Examples 4-5, it can be seen that the cycle performance and first discharge specific capacity of the lithium-ion battery prepared by limiting the molar ratio of the iron element in the iron-based metal-organic framework material to the manganese element in the manganese-based metal-organic framework material within the preferred range are further improved.

[0095] Comparing Example 1 with Examples 8-9, it can be seen that the cycle performance and first discharge specific capacity of the lithium-ion battery prepared by limiting the two-step sintering temperature to a preferred range in Example 1 are further improved.

[0096] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A method for preparing lithium manganese iron phosphate, characterized in that: The steps include: Step S1: mixing a manganese source and an iron source to obtain a first mixture; at least one of the manganese source and the iron source is a metal organic framework material; Step S2: sintering the first mixture at 300-1200° C. to obtain ferromanganese oxide; Step S3: mixing the manganese iron oxide with the lithium source, the phosphorus source and the carbon source and drying the mixture to obtain a second mixture; Step S4: sintering the second mixture at 500-900° C. to obtain lithium manganese iron phosphate.

2. The method for preparing lithium iron manganese phosphate according to claim 1, characterized in that: The manganese source is one or more of manganese-based metal organic framework materials, elemental manganese, manganese tetraoxide, manganese trioxide, manganous oxide, manganese oxide, manganese dioxide, monohydroxy manganese oxide MnO(OH), hydrated manganese dioxide MnO(OH)2, manganese hydroxide Mn(OH)2, manganese carbonate, manganese sulfate, manganese nitrate, manganese citrate, manganese oxalate, manganese formate, manganese acetate, and manganese phosphate.

3. The method for preparing lithium manganese iron phosphate according to claim 2, characterized in that: The manganese-based metal organic framework material is composed of a manganese salt and an organic ligand connected by a coordination bond; preferably, the manganese salt is MnCl2·4H2O, and the organic ligand is 2,5-dihydroxyterephthalic acid.

4. The method for preparing lithium manganese iron phosphate according to claim 1, characterized in that: The iron source is one or more of an iron-based metal organic framework material, elemental iron, ferroferric oxide, ferrous oxide, basic iron oxide FeO(OH), ferric hydroxide, ferrous hydroxide, ferrous sulfate, ferric sulfate, ferric nitrate, ferric nitrate nonahydrate, ferrous nitrate, ferrous chloride, ferric bromide, ferric phosphate, ferrous phosphate, ferrous carbonate, ferric oxalate, ferrous oxalate, ferrous acetate, ferric citrate, and ferrous citrate.

5. The method for preparing lithium iron manganese phosphate according to claim 4, characterized in that: The iron-based metal organic framework material is composed of an iron salt and an organic ligand connected by a coordination bond; preferably, the iron salt is FeCl3·6H2O, and the organic ligand is terephthalic acid.

6. The method for preparing lithium manganese iron phosphate according to any one of claims 1 to 5, characterized in that: In step S1, the molar ratio of the iron element in the iron source to the manganese element in the manganese source is 1:9-9:1, preferably 4:

6.

7. The method for preparing lithium manganese iron phosphate according to any one of claims 1 to 6, characterized in that: The molecular formula of the lithium iron manganese phosphate is: LiMn x Fe 1-x PO4, wherein 0<x<1; and / or, the lithium source is one or more of lithium carbonate, lithium hydroxide, lithium oxide, lithium peroxide, lithium bicarbonate, lithium phosphate, lithium dihydrogen phosphate, dilithium hydrogen phosphate, lithium oxalate, lithium acetate, lithium sulfate, lithium nitrate, lithium chloride, lithium sulfide, lithium citrate, lithium benzoate, lithium borate, lithium metaborate, and lithium tetrachloroborate; and / or, the phosphorus source is one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium tripolyphosphate, phosphoric acid, calcium phosphate, phosphate ester, lithium dihydrogen phosphate, iron phosphate, lithium phosphate, lithium dihydrogen phosphate, and manganese phosphate.

8. The method for preparing lithium manganese iron phosphate according to claim 1, characterized in that: The carbon source is one or more of glucose, citric acid, urea, melamine, sodium gluconate, sodium citrate, polyethylene glycol, soybean meal, fructose, starch, phenolic resin, and vitamin C; and / or the ratio of the molar amount of the carbon source to the molar amount of the lithium source is 1:5-1:

50.

9. A positive electrode material, characterized in that: The invention relates to lithium manganese iron phosphate prepared by the preparation method described in any one of claims 1 to 8.

10. A lithium ion battery, characterized in that: It comprises a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator, wherein the positive electrode sheet is made of the positive electrode material according to claim 9.

Citation Information

Patent Citations

  • Carbon-coated lithium iron phosphate composite material, preparation method thereof and lithium ion battery

    CN111430687A

  • Preparation method for synthesizing doped lithium manganese phosphate / carbon composite material based on mixed metal organic framework

    CN112952058A

  • Composite positive electrode material and preparation method and application thereof

    CN115893363A

  • Positive electrode active material precursor and preparation method thereof

    CN116354327A

  • Preparation method of lithium manganese iron phosphate, positive electrode material and lithium ion battery

    CN116969435A

Cited By

  • Preparation method of boron-doped coated lithium iron manganese phosphate positive electrode material and lithium battery

    CN119390039A

  • Preparation method of boron-doped coated lithium manganese iron phosphate positive electrode material and lithium battery

    CN119390039B

  • Lithium manganese iron phosphate positive electrode material as well as preparation method and application thereof

    CN119674038A

  • Lithium manganese iron phosphate composite material and preparation method thereof

    CN122426723A