Medium-band-gap fused ring acceptor material, preparation method thereof and application of medium-band-gap fused ring acceptor material to photovoltaic device
By using alkoxy side chain and thiophene structure and weak electron-absorbing end groups in organic solar cells and indoor photovoltaic devices, the problem of lack of medium band gap acceptor materials in the prior art is solved. High efficiency device performance and excellent photoelectric characteristics are achieved.
Patent Information
- Application Number
- CN202310590462.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-26
AI Technical Summary
The lack of efficient medium bandgap acceptor materials in existing organic solar cells limits the improvement of device performance and efficiency, especially in stacked structures and indoor photovoltaic applications.
The medium band gap fused ring acceptor material containing alkoxy side chain n-thiophene structure and weak electron-absorbing end groups is prepared through a specific synthetic route for the preparation of the material as an acceptor in organic solar cells and indoor photovoltaic devices. High-efficiency device performance and excellent photoelectric characteristics.
High-efficiency stacked organic solar cells and indoor photovoltaic devices are achieved, with significant improvement in open circuit voltage and filling factors, with efficiency exceeding 20% and 31%, and good light absorption complementary and voltage superposition effects are demonstrated.
Smart Images

Figure CN119019422A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of organic solar cell material preparation, relates to a class of organic solar cell receptor materials, specifically to a class of medium bandgap receptor materials containing a condensed ring structure, and also to applications in laminated organic solar cells and indoor photovoltaic devices. Background Art
[0002] With the extensive use of fossil energy, environmental pollution and energy depletion are becoming increasingly serious, and the development of new clean energy is imminent. Solar energy has attracted widespread attention due to its many advantages such as clean, pollution-free, inexhaustible and inexhaustible. Better use of solar energy is an effective solution to the energy crisis. A solar cell is a device that can directly convert light energy into electrical energy. Past studies have found that organic solar cells (OSCs) are favored by researchers because of their low manufacturing cost, good mechanical flexibility and light weight. Thanks to the continuous innovation of active layer materials, especially the development of non-fullerene acceptors (NFAs), organic solar cells have developed rapidly, and their power conversion efficiency has now exceeded 19% (Adv. Mater., 2021, 33, e2102420; Joule., 2022, 6, 171-184).
[0003] Although the efficiency of OSCs devices (over 19%) has been greatly improved, there is still a significant gap compared with commercial silicon-based solar cells and high-efficiency perovskite solar cells. Theory and experiments show that stacked organic solar cells are a feasible way to further improve the efficiency of OSCs. Fig.12a As shown, stacked organic cells can utilize two (a front cell with wide bandgap absorption and a rear cell with narrow bandgap absorption) or multiple active layers with complementary absorption to broaden the absorption range, thereby being able to utilize photons in various bands to a greater extent. Among them, acceptor materials with narrow bandgap absorption characteristics have been widely studied, and device performance has also made great progress. However, the research on medium-bandgap acceptor materials for the preparation of high-efficiency front cells is still lagging behind, and there is an urgent need to develop excellent medium-bandgap acceptor materials to improve the performance of the front cell. In addition, due to the advantages of flexible and adjustable material structure and absorption range, OSCs have unique advantages in some special application scenarios. Such as Figure 12b As shown in the figure, in indoor environments, the absorption spectrum of medium-bandgap materials has a high degree of match with the emission spectrum of indoor light sources, so indoor photovoltaic devices based on medium-bandgap acceptor materials can effectively utilize indoor light. Such devices can power small instruments such as wearable devices and IoT devices, which can greatly promote the development of intelligent devices and the IoT industry.
[0004] Since XW Zhan et al. discovered condensed-ring NFAs in 2015, this type of material has attracted great interest from researchers. With the continuous efforts of researchers, the material structure has been continuously innovated and the device performance has been rapidly improved. In order to obtain the highest possible photocurrent to achieve efficiency breakthroughs, researchers generally favor acceptor materials with near-infrared absorption (narrow band gap). However, medium band gap (E) with spectral absorption edge in the range of 600–800nm is not suitable for photocurrents. g ≈1.55–2.00eV) acceptor materials have unique advantages in tandem organic cells and indoor photovoltaics. However, this type of material has received less attention and is very scarce. Through literature research, it was found that there are few studies on medium-bandgap acceptors, with only a few literature reports (Adv. Mater. 2017, 29, 1700254; Chem. Mater. 2019, 31, 3941-3947; Energy Environ. Sci., 2020, 13, 2864; Joule. 2021, 5, 1231-1245; Adv. Mater. 2022, 34, 2108090), and the efficiency is generally not high. Therefore, in order to promote the efficiency improvement and commercial application of organic solar cells, we invented a class of medium-bandgap fused ring acceptors to achieve high-efficiency tandem organic solar cells and indoor photovoltaic devices. Summary of the invention
[0005] The purpose of the present invention is to prepare a medium band gap (E g ≈1.55–2.00eV) fused ring acceptor materials can be used as acceptors in the active layer of OSCs. Such materials have the advantages of high lowest unoccupied molecular orbital energy level (LUMO), absorption range from near ultraviolet to visible light, and high device open circuit voltage. When used as acceptor materials in tandem organic solar cells and indoor photovoltaic devices, they can show excellent device performance, high open circuit voltage and fill factor. Therefore, such materials have good application prospects in the field of tandem organic solar cells and indoor photovoltaic devices.
[0006] The technical solution adopted by the present invention is to provide a medium band gap condensed ring receptor material using both an alkoxy side chain structure and a weak electron-withdrawing end group structure. The structural feature of the condensed ring central core is that the condensed ring center is composed of a thiophene conjugated unit containing an alkoxy side chain and other conjugated structures, and the two sides of the central core are connected to the weak electron-withdrawing end groups. The general structural formula is shown in Formula I:
[0007]
[0008] in:
[0009] In the structural formula, R1 and R2 are independently selected from a linear, branched or alkyl-substituted aromatic chain having 1 to 40 carbon atoms;
[0010] The Weak A unit is selected from any one of the following structural formulas:
[0011]
[0012] in:
[0013] The dotted line in the Weak A structure indicates the connection site to the Weak A unit.
[0014] Further, the Ar1 unit is selected from any one of the following structural formulas:
[0015]
[0016] Wherein, R3 in the Ar1 structural formula is independently selected from H, a linear, branched or alkyl-substituted aromatic chain having 1 to 20 carbon atoms, and the dotted line in the Ar1 structural formula represents the connection site with other units.
[0017] A method for preparing a medium-bandgap fused-ring receptor material comprises the following steps:
[0018] Its synthetic route is as follows:
[0019]
[0020] In the structural formula, R1 and R2 are both straight chain, branched chain or alkyl-substituted aromatic side chains having 1 to 40 carbon atoms.
[0021] (1) Compound A and Compound B are added to 80-100 mL of toluene, and catalysts tri(dibenzylideneacetone)dipalladium and tri(o-methylphenyl)phosphine are added, and the reaction is carried out at 80-85° C. for 4-6 hours to obtain Compound C through Stille coupling reaction;
[0022] (2) Under nitrogen protection, compound C and triphenylphosphine are added to o-dichlorobenzene, heated to 160-180° C. for reaction for 15-18 hours to obtain compound D;
[0023] (3) Under nitrogen protection, compound D, alkyl halide (R2-Br), potassium carbonate and potassium iodide are added to N,N-dimethylformamide, and reacted at 80-85° C. for 10-12 h to obtain compound E;
[0024] (4) This reaction is a Vilsmeier-Haack reaction. Under nitrogen protection, compound E is dissolved in 1,2-dichloroethane, and then added dropwise to the formylation reagent phosphorus oxychloride at -10 to 0°C, with the molar ratio of compound E to phosphorus oxychloride being 1:10 to 1:30. After reacting at -10 to 0°C for 1 to 2 hours, the system is heated to 80 to 100°C and reacted for 8 to 12 hours to obtain compound F.
[0025] (5) This reaction is a Knoevenagel condensation reaction. Under nitrogen protection, compound F is reacted with pyridine at 60-65°C for 5-8h to obtain compound G.
[0026] Compared with the prior art, the present invention has the following advantages:
[0027] (1) The present invention firstly utilizes the synergistic effect of the alkoxy side chain thiophene structure and the weak electron-withdrawing end group to obtain a medium band gap (E) with a high absorption coefficient. g ≈1.55-2.00eV) fused ring acceptor materials, whose absorption range is in the near-ultraviolet and visible light regions, are significantly blue-shifted compared to common narrow-bandgap acceptor materials.
[0028] (2) Compared with the three reported combination types of materials, namely, alkyl side chain-strong electron-withdrawing end group, alkoxy side chain-strong electron-withdrawing end group, and alkyl side chain-weak electron-withdrawing end group, this type of material has a higher LUMO energy level, thereby significantly improving the open-circuit voltage of photovoltaic devices.
[0029] (3) The light absorption range of this type of material is complementary to that of the narrow-bandgap acceptor material and can provide a higher open-circuit voltage. When used as a front cell, it can achieve good light absorption complementarity and voltage superposition with the rear cell made of a narrow-bandgap acceptor material, thereby realizing a high-efficiency stacked organic solar cell (efficiency exceeding 20%).
[0030] (4) The light absorption range of this type of material has a good match with the emission spectrum of indoor lighting sources. Photovoltaic devices based on this type of receptor material exhibit excellent open-circuit voltage and energy conversion efficiency (efficiency exceeding 31%) under indoor light irradiation, and have important applications in indoor photovoltaic devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is the thin film absorption spectrum of the acceptor molecule YO4Cl-BO.
[0032] Figure 2 This is the thin film absorption spectrum of the receptor molecule YOS-BO.
[0033] Figure 3 This is the thin film absorption spectrum of the acceptor molecule YOSCl-BO.
[0034] Figure 4 This is the thin film absorption spectrum of the acceptor molecule YOFN-BO.
[0035] Figure 5 This is the thin film absorption spectrum of the acceptor molecule YO4Cl-Se.
[0036] Figure 6 This is the thin film absorption spectrum of the receptor molecule YON-EH.
[0037] Figure 7 This is the thin film absorption spectrum of the acceptor molecule YO4Cl-Dq.
[0038] Figure 8 J–V characteristic curves of PBDB-T as donor and YO4Cl-BO, YO4Cl-Se and YO4Cl-Dq as acceptors.
[0039] Fig. 9 EQE characteristic curves with PBDB-T as donor and YO4Cl-BO, YO4Cl-Se and YO4Cl-Dq as acceptors.
[0040] Fig.10 The J–V characteristic curves of the stacked cells prepared with PM6:Y6-BO / Y6-O / BTP-S3 and PBDB-T:YO4Cl-Se as the front cells and PTTzF:Y6:
[70] PCBM as the back cells.
[0041] Fig.11 J–V characteristic curves of single junction devices based on PM6:Y6-BO / Y6-O / BTP-S3 and PBDB-T:YO4Cl-Se under indoor lighting conditions.
[0042] Fig.12a It is a stacked battery device structure;
[0043] Figure 12b These are the luminous spectra of AM 1.5G, FL2700 K and LED 2700K light sources. DETAILED DESCRIPTION
[0044] In order to make the purpose, technical solution and advantages of the present invention more clear, the specific implementation of the present invention is further described below with reference to the accompanying drawings and examples, but the implementation and protection of the present invention are not limited thereto. It should be pointed out that if there are processes that are not particularly described in detail below, they can be implemented or understood by those skilled in the art with reference to the prior art.
[0045] The practice of the present invention can adopt conventional techniques of organic synthetic chemistry and organic photovoltaic device preparation. In the following examples, efforts are made to ensure the accuracy of the numbers used (including mass, temperature, time, etc.), but some experimental errors and deviations should be considered. The temperatures used in the following examples are expressed in ° C, and the pressure is atmospheric pressure or near atmospheric pressure. The solvents used are analytically pure or chromatographically pure, all reactions are carried out in an inert gas atmosphere, and the device preparation is carried out in a nitrogen glove box. Unless otherwise indicated, all reagents are obtained through commercial channels.
[0046] Example 1
[0047]
[0048] (1) Raw materials or intermediate reactants
[0049] Triphenylphosphine, tris(dibenzylideneacetone)dipalladium (Pd2(dba)3), tri(o-methylphenyl)phosphine (P(o-tol)3), 5-(bromomethyl)undecane, potassium carbonate (K2CO3), potassium iodide (KI), pyridine, phosphorus oxychloride (POCl3), N,N-dimethylformamide (DMF), 1,2-dichloroethane, tetrahydrofuran (THF), toluene, chlorobenzene and chloroform were purchased from companies such as Anage, Bailingwei and Suzhou Nakai.
[0050] (2) Preparation of Compound 3
[0051] Compound 1 (4,7-dibromo-5,6-dinitrobenzo[c][1,2,5]thiadiazole) (3.82 g, 10 mmol), compound 2 (17.58 g, 30 mmol), Pd2(dba)3 (172.5 mg, 0.3 mmol), and P(o-tol)3 (377.4 mg, 1.24 mmol) were added to toluene (60 mL) under nitrogen. The reaction mixture was heated to reflux and stirred for 13 h. After the reaction solution was cooled to room temperature, the reaction was quenched with water and extracted with dichloromethane. The organic phase was concentrated under reduced pressure to obtain a crude product, which was purified by silica gel column chromatography using a mixed solvent of petroleum ether and dichloromethane as the eluent (V / V=3:1) to obtain compound 3 (the product was a red solid of 7.18 g, yield=88.2%).
[0052] (3) Synthesis of Compound 4
[0053] Under nitrogen atmosphere, compound 3 (3.25 g, 4 mmol) and PPh3 (10.48 g, 40 mmol) were added to 20 mL o-dichlorobenzene (o-DCB). The reaction system was heated to reflux and reacted for 18 h. After the reaction was completed, it was cooled to room temperature, and then the solvent was removed under reduced pressure and precipitated with 100 mL of methanol. The crude product was filtered and used directly in the next reaction. The crude product, 5-(bromomethyl)undecane (4.53 g, 18.16 mmol), KI (0.75 g, 4.54 mmol), and K2CO3 (5.92 g, 18.16 mmol) were added to 50 mL of DMF. Under nitrogen atmosphere, the reaction was stirred at 80 ° C for 24 h. After cooling to room temperature, the reaction was quenched with water and extracted with dichloromethane. The combined organic phase was further washed with water, dried over anhydrous MgSO4, filtered and concentrated under reduced pressure. The product was purified by silica gel column chromatography using a mixed solvent of petroleum ether and dichloromethane as eluent (V / V=6:1) to obtain compound 4 (yellow oily liquid 2.42 g, yield=55.7%).
[0054] (4) Synthesis of Compound 5
[0055] In a nitrogen atmosphere, POCl3 (3.06 g, 20 mmol) was slowly added to anhydrous DMF (1.1 g, 15 mmol) at 0°C, and the mixture was stirred for 2 h. 25 mL of 1,2-dichloroethane containing compound 4 (1.2 g, 1 mmol) was slowly added dropwise to the reaction solution, stirred at 0°C for 1 h, and then heated to 90°C for 12 h. After the reaction was completed, the mixture was cooled to room temperature, extracted with dichloromethane, and the organic phase was dried over anhydrous MgSO4 and filtered. The organic solvent was removed, and the crude product was separated by column chromatography using a mixed solvent of petroleum ether and dichloromethane as the eluent (V / V=1:2) to obtain compound 5 (0.86 g of yellow solid, yield=75.4%).
[0056] (5) Compound YO4Cl-BO
[0057] Under nitrogen atmosphere, compound 5 (300 mg), compound 6 (369 mg), and 30 mL of chloroform were added to a 100 mL two-necked flask, and 1 mL of pyridine was added, and the mixture was stirred at 65°C for 24 h. After the reaction solution was cooled to room temperature, methanol was used for precipitation, and the precipitate was collected by filtration. The crude product was separated by column chromatography using a mixed solvent of petroleum ether and dichloromethane as the eluent (V / V=1:1) to obtain a black solid (368 mg, yield=84.2%).
[0058] Example 2
[0059]
[0060] (1) Raw materials or intermediate reactants
[0061] Triphenylphosphine, tris(dibenzylideneacetone)dipalladium (Pd2(dba)3), tri(o-methylphenyl)phosphine (P(o-tol)3), 5-(bromomethyl)undecane, potassium carbonate (K2CO3), potassium iodide (KI), pyridine, phosphorus oxychloride (POCl3), N,N-dimethylformamide (DMF), 1,2-dichloroethane, tetrahydrofuran (THF), toluene, chlorobenzene and chloroform were purchased from companies such as Anage, Bailingwei and Suzhou Nakai.
[0062] (2) The preparation of compound 3, compound 4 and compound 5 is the same as YO4Cl-BO.
[0063] (3) Compound YOS-BO
[0064] Under nitrogen atmosphere, compound 5 (300 mg), compound 7 (240 mg), and 30 mL of chloroform were added to a 100 mL two-necked flask, and 1 mL of pyridine was added, and the mixture was stirred at 65°C for 24 h. After the reaction solution was cooled to room temperature, it was precipitated with methanol, filtered, and the precipitate was collected. The crude product was separated by column chromatography, and the eluent was PE:DCM=1:1, to obtain compound YOS-BO (black solid 314 mg, yield=86.2%).
[0065] Example 3
[0066]
[0067] (1) Raw materials or intermediate reactants
[0068] Triphenylphosphine, tris(dibenzylideneacetone)dipalladium (Pd2(dba)3), tri(o-methylphenyl)phosphine (P(o-tol)3), 5-(bromomethyl)undecane, potassium carbonate (K2CO3), potassium iodide (KI), pyridine, phosphorus oxychloride (POCl3), N,N-dimethylformamide (DMF), 1,2-dichloroethane, tetrahydrofuran (THF), toluene, chlorobenzene and chloroform were purchased from companies such as Anage, Bailingwei and Suzhou Nakai.
[0069] (2) The preparation of compound 3, compound 4 and compound 5 is the same as YO4Cl-BO.
[0070] (3) Synthesis of compound YOSCl-BO
[0071] Under nitrogen atmosphere, compound 5 (300 mg), compound 8 (307 mg), and 30 mL of chloroform were added to a 100 mL two-necked flask, and 1 mL of pyridine was added. The mixture was stirred at 65°C for 24 h. After the reaction solution was cooled to room temperature, methanol was used for precipitation, filtration, and the precipitate was collected. The crude product was separated by column chromatography. A mixed solvent of petroleum ether and dichloromethane was used as the eluent (V / V=1:1) to obtain a black solid (358 mg, yield=86.6%).
[0072] Example 4
[0073]
[0074] (1) Raw materials or intermediate reactants
[0075] Triphenylphosphine, tris(dibenzylideneacetone)dipalladium (Pd2(dba)3), tri(o-methylphenyl)phosphine (P(o-tol)3), 5-(bromomethyl)undecane, potassium carbonate (K2CO3), potassium iodide (KI), pyridine, phosphorus oxychloride (POCl3), N,N-dimethylformamide (DMF), 1,2-dichloroethane, tetrahydrofuran (THF), toluene, chlorobenzene and chloroform were purchased from companies such as Anage, Bailingwei and Suzhou Nakai.
[0076] (2) The preparation of compound 3, compound 4 and compound 5 is the same as YO4Cl-BO.
[0077] (3) Synthesis of compound YOFN-BO
[0078] Under nitrogen atmosphere, compound 5 (300 mg), compound 9 (257 mg), and 30 mL of chloroform were added to a 100 mL two-necked flask, and 1 mL of pyridine was added. The mixture was stirred at 65 ° C for 24 h. After the reaction solution was cooled to room temperature, methanol was used for precipitation, filtration, and the precipitate was collected. The crude product was separated by column chromatography. A mixed solvent of petroleum ether and dichloromethane was used as the eluent (V / V=3:1) to obtain a black solid (304 mg, yield=77.4%).
[0079] Example 5
[0080]
[0081] (1) Raw materials or intermediate reactants
[0082] Triphenylphosphine, tris(dibenzylideneacetone)dipalladium (Pd2(dba)3), tri(o-methylphenyl)phosphine (P(o-tol)3), 5-(bromomethyl)undecane, potassium carbonate (K2CO3), potassium iodide (KI), pyridine, phosphorus oxychloride (POCl3), N,N-dimethylformamide (DMF), 1,2-dichloroethane, tetrahydrofuran (THF), toluene, chlorobenzene and chloroform were purchased from companies such as Anage, Bailingwei and Suzhou Nakai.
[0083] (2) Preparation of Compound 11
[0084] Compound 10 (4,7-dibromo-5,6-dinitrobenzo[c][1,2,5]selenadiazole) (4.30 g, 10 mmol), compound 2 (17.58 g, 30 mmol), Pd2(dba)3 (172.5 mg, 0.3 mmol) and P(o-tol)3 (377.4 mg, 1.24 mmol) were added to toluene (60 mL) under nitrogen. The reaction mixture was heated to reflux and stirred for 13 h. After the reaction solution was cooled to room temperature, the reaction was quenched with water and extracted with dichloromethane. The organic phase was concentrated under reduced pressure to obtain a crude product, which was purified by silica gel column chromatography using a mixed solvent of petroleum ether and dichloromethane as the eluent (V / V=2:1) to obtain compound 11 (the product was a red solid of 7.30 g, yield=84.7%).
[0085] (3) Synthesis of Compound 12
[0086] Under nitrogen atmosphere, compound 11 (3.45 g, 4 mmol) and PPh3 (10.48 g, 40 mmol) were added to 20 mL o-DCB. The reaction system was heated to reflux and reacted for 18 h. After the reaction was completed, it was cooled to room temperature, the solvent was removed under reduced pressure, and 100 mL of methanol was used for precipitation. The crude product was filtered and used directly in the next step. The crude product, 5-(bromomethyl)undecane (4.53 g, 18.16 mmol), KI (0.75 g, 4.54 mmol), and K2CO3 (5.92 g, 18.16 mmol) were added to 50 mL DMF. Under nitrogen conditions, the reaction was stirred at 80 ° C for 24 h. After cooling to room temperature, the reaction was quenched with water and extracted with dichloromethane. The combined organic phase was further washed with water, dried over anhydrous MgSO4, filtered and concentrated under reduced pressure. The product was purified by silica gel column chromatography using a mixed solvent of petroleum ether and dichloromethane as eluent (V / V=5:1) to obtain compound 12 (yellow oily liquid 2.42 g, yield=53.4%).
[0087] (4) Synthesis of Compound 13
[0088] In a nitrogen atmosphere, POCl3 (3.06 g, 20 mmol) was slowly added to anhydrous DMF (1.1 g, 15 mmol) at 0°C and the mixture was kept warm for 2 h. 25 mL of 1,2-dichloroethane containing compound 12 (1.1 g, 1 mmol) was slowly added dropwise to the reaction solution, stirred at 0°C for 1 h, and then heated to 90°C for 12 h. After the reaction was completed, the mixture was cooled to room temperature and extracted with dichloromethane. The organic phase was dried over anhydrous MgSO4 and filtered. The organic solvent was removed, and the crude product was separated by column chromatography using a mixed solvent of petroleum ether and dichloromethane as the eluent (V / V=1:2) to obtain compound 13 (0.97 g yellow solid, yield=81.6%).
[0089] (5) Compound YO4Cl-Se
[0090] Under nitrogen atmosphere, compound 13 (312 mg), compound 6 (369 mg), and 30 mL of chloroform were added to a 100 mL two-necked flask, and 1 mL of pyridine was added. The mixture was stirred at 65°C for 24 h. After the reaction solution was cooled to room temperature, methanol was used for precipitation, filtration, and the precipitate was collected. The crude product was separated by column chromatography. A mixed solvent of petroleum ether and dichloromethane was used as the eluent (V / V=1:1) to obtain a black solid (370 mg, yield=82.2%).
[0091] Example 6
[0092]
[0093] (1) Raw materials or intermediate reactants
[0094] Triphenylphosphine, tris(dibenzylideneacetone)dipalladium (Pd2(dba)3), tri(o-methylphenyl)phosphine (P(o-tol)3), 5-(bromomethyl)undecane, potassium carbonate (K2CO3), potassium iodide (KI), pyridine, phosphorus oxychloride (POCl3), N,N-dimethylformamide (DMF), 1,2-dichloroethane, tetrahydrofuran (THF), toluene, chlorobenzene and chloroform were purchased from companies such as Anage, Bailingwei and Suzhou Nakai.
[0095] (2) Preparation of Compound 15
[0096] Compound 14 (4,7-dibromo-2-(2-ethylhexyl)-5,6-dinitro-2H-benzo[D][1,2,3]triazole) (4.77 g, 10 mmol), compound 2 (17.58 g, 30 mmol), Pd2(dba)3 (172.5 mg, 0.3 mmol), and P(o-tol)3 (377.4 mg, 1.24 mmol) were added to a toluene (60 mL) solution under nitrogen. The reaction mixture was heated to reflux and stirred for 13 h. After the reaction solution was cooled to room temperature, the reaction was quenched with water and extracted with dichloromethane. The organic phase was concentrated under reduced pressure to obtain a crude product, which was purified by silica gel column chromatography using a mixed solvent of petroleum ether and dichloromethane as an eluent (V / V=3:1) to obtain compound 15 as a red solid (7.75 g, yield=85.2%).
[0097] (3) Synthesis of Compound 16
[0098] Under nitrogen atmosphere, compound 15 (3.10 g, 4 mmol) and PPh3 (10.48 g, 40 mmol) were added to 20 mL o-DCB. The reaction system was heated to reflux and reacted for 18 h. After the reaction was completed, it was cooled to room temperature, the solvent was removed under reduced pressure, and 100 mL of methanol was used for precipitation. The crude product was filtered and used directly in the next step. The crude product, 5-(bromomethyl)undecane (4.53 g, 18.156 mmol), KI (0.75 g, 4.54 mmol), and K2CO3 (5.92 g, 18.16 mmol) were added to 50 ml of DMF. Under nitrogen conditions, the reaction was stirred at 80 ° C for 24 h. After cooling to room temperature, the reaction was quenched with water and extracted with dichloromethane. The combined organic phase was further washed with water, dried over anhydrous MgSO4, filtered and concentrated under reduced pressure. The product was purified by silica gel column chromatography using a mixed solvent of petroleum ether and dichloromethane as eluent (V / V=8:1) to obtain compound 16 (yellow oily liquid 2.27 g, yield = 48.0%).
[0099] (4) Synthesis of Compound 17
[0100] In a nitrogen atmosphere, POCl3 (3.06 g, 20 mmol) was slowly added to anhydrous DMF (1.1 g, 15 mmol) at 0°C and the mixture was kept warm for 2 h. 25 mL of 1,2-dichloroethane containing compound 16 (1.18 g, 1 mmol) was slowly added dropwise to the reaction solution, stirred at 0°C for 1 h, and then heated to 90°C for 12 h. After the reaction was completed, the mixture was cooled to room temperature and extracted with DCM. The organic phase was dried over anhydrous MgSO4 and filtered. The organic solvent was removed, and the crude product was separated by column chromatography using a mixed solvent of petroleum ether and dichloromethane as the eluent (V / V=1:1) to obtain compound 17 (0.98 g yellow solid, yield=79.3%).
[0101] (5) Compound YON-EH
[0102] Under nitrogen atmosphere, compound 17 (300 mg), compound 7 (240 mg), and 30 mL of chloroform were added to a 100 ml two-necked flask, and 1 mL of pyridine was added. The mixture was stirred at 65 °C for 24 h. After the reaction solution was cooled to room temperature, methanol was used for precipitation, filtration, and the precipitate was collected. The crude product was separated by column chromatography. The eluent was PE:DCM = 1:1, and compound YON-EH (black solid 342 mg, yield = 88.2%) was obtained.
[0103] Example 9
[0104]
[0105] (1) Raw materials or intermediate reactants
[0106] Triphenylphosphine, tris(dibenzylideneacetone)dipalladium (Pd2(dba)3), tri(o-methylphenyl)phosphine (P(o-tol)3), 5-(bromomethyl)undecane, potassium carbonate (K2CO3), potassium iodide (KI), pyridine, phosphorus oxychloride (POCl3), N,N-dimethylformamide (DMF), 1,2-dichloroethane, tetrahydrofuran (THF), toluene, chlorobenzene and chloroform were purchased from companies such as Anage, Bailingwei and Suzhou Nakai.
[0107] (2) Preparation of Compound 19
[0108] Compound 18 (5,8-dibromo-6,7-dinitroquinoxaline) (3.76 g, 10 mmol), compound 2 (17.58 g, 30 mmol), Pd2(dba)3 (172.5 mg, 0.3 mmol), and P(o-tol)3 (377.4 mg, 1.24 mmol) were added to toluene (60 mL) under nitrogen. The reaction mixture was heated to reflux and stirred for 13 h. After the reaction solution was cooled to room temperature, the reaction was quenched with water and extracted with dichloromethane. The organic phase was concentrated under reduced pressure to obtain a crude product, which was purified by silica gel column chromatography using a mixed solvent of petroleum ether and dichloromethane as an eluent (V / V=2:1) to obtain compound 19 (the product was a red solid of 6.66 g, yield=82.4%).
[0109] (3) Synthesis of Compound 20
[0110] Under nitrogen atmosphere, compound 19 (3.45 g, 4 mmol) and PPh3 (10.48 g, 40 mmol) were added to 20 mL o-DCB. The reaction system was heated to reflux and reacted for 18 h. After the reaction was completed, it was cooled to room temperature, the solvent was removed under reduced pressure, and 100 mL of methanol was used for precipitation. The crude product was filtered and used directly in the next step. The crude product, 5-(bromomethyl)undecane (4.53 g, 18.16 mmol), KI (0.75 g, 4.54 mmol), and K2CO3 (5.92 g, 18.16 mmol) were added to 50 mL DMF. Under nitrogen conditions, the reaction was stirred at 80 ° C for 24 h. After cooling to room temperature, the reaction was quenched with water and extracted with dichloromethane. The combined organic phase was further washed with water, dried over anhydrous MgSO4, filtered and concentrated under reduced pressure. The product was purified by silica gel column chromatography using a mixed solvent of petroleum ether and dichloromethane as eluent (V / V=3:1) to obtain compound 20 (yellow oily liquid 2.15 g, yield = 49.7%).
[0111] (4) Synthesis of Compound 21
[0112] In a nitrogen atmosphere, POCl3 (3.06 g, 20 mmol) was slowly added to anhydrous DMF (1.1 g, 15 mmol) at 0°C and the mixture was kept warm for 2 h. 25 mL of 1,2-dichloroethane containing compound 20 (1.08 g, 1 mmol) was slowly added dropwise to the reaction solution, stirred at 0°C for 1 h, and then heated to 90°C for 12 h. After the reaction was completed, the mixture was cooled to room temperature, extracted with dichloromethane, and the organic phase was dried over anhydrous MgSO4 and filtered. The organic solvent was removed and the crude product was separated by column chromatography. A mixed solvent of petroleum ether and dichloromethane was used as the eluent (V / V=1:2) to obtain compound 21 (0.95 g yellow solid, yield=83.3%).
[0113] (5) Compound YO4Cl-Dq
[0114] Under nitrogen atmosphere, compound 21 (300 mg), compound 6 (373 mg), and 30 mL of chloroform were added to a 100 mL two-necked flask, and 1 mL of pyridine was added. The mixture was stirred at 65 ° C for 24 h. After the reaction solution was cooled to room temperature, methanol was used for precipitation, filtration, and the precipitate was collected. The crude product was separated by column chromatography. A mixed solvent of petroleum ether and dichloromethane was used as the eluent (V / V=1:1) to obtain YO4Cl-Dq (black solid 370 mg, yield=84.2%).
[0115] Example 10
[0116] Figure 1This is the UV-visible absorption spectrum of the compound YO4Cl-BO film. In the range of 300-900nm, the absorption peak of the compound YO4Cl-BO is located at 677nm, the optical absorption edge is 731nm, and the corresponding optical band gap is 1.70eV.
[0117] Figure 2 This is the UV-visible absorption spectrum of the compound YOS-BO film. In the range of 300-900 nm, the absorption peak of the compound YOS-BO is located at 700 nm, while the optical absorption edge is 756 nm, and the corresponding optical band gap is 1.64 eV.
[0118] Figure 3 This is the UV-visible absorption spectrum of the compound YOSCl-BO film. In the range of 300-900 nm, the absorption peak of the compound YOSCl-BO is located at 707 nm, the optical absorption edge is 765 nm, and the corresponding optical band gap is 1.62 eV.
[0119] Figure 4 This is the UV-visible absorption spectrum of the compound YOFN-BO film. In the range of 300-900nm, the absorption peak of the compound YOFN-BO is located at 677nm, the optical absorption edge is 725nm, and the corresponding optical band gap is 1.71eV.
[0120] Figure 5 This is the UV-visible absorption spectrum of the compound YO4Cl-Se film. In the range of 300-900nm, the absorption peak of the compound YO4Cl-Se is located at 686nm, the optical absorption edge is 741nm, and the corresponding optical band gap is 1.67eV.
[0121] Figure 6 This is the UV-visible absorption spectrum of the compound YON-EH film. In the range of 300-900nm, the absorption peak of the compound YON-EH is located at 721nm, the optical absorption edge is 783nm, and the corresponding optical band gap is 1.58eV.
[0122] Figure 7 This is the UV-visible absorption spectrum of the compound YO4Cl-Dq film. In the range of 300-900nm, the absorption peak of the compound YO4Cl-Dq is located at 684nm, the optical absorption edge is 720nm, and the corresponding optical band gap is 1.72eV.
[0123] Figure 8JV curves of organic solar cell devices based on PBDB-T:YO4Cl-Dq, PBDB-T:YO4Cl-BO and PBDB-T:YO4Cl-Se. The PBDB-T:YO4Cl-Dq device exhibited an open circuit voltage of 1.14 volts, a short circuit current of 14.72 mA / cm2 and a fill factor of 77.56%. Finally, an efficiency of 13.01% was achieved. The PBDB-T:YO4Cl-BO device exhibited an open circuit voltage of 1.12 volts, a short circuit current of 15.72 mA / cm2 and a fill factor of 78.25%. Finally, an efficiency of 13.77% was achieved. The PBDB-T:YO4Cl-Se device exhibited an open circuit voltage of 1.11 volts, a short circuit current of 15.94 mA / cm2 and a fill factor of 79.69%. Finally, an efficiency of 14.10% was achieved.
[0124] Fig. 9 The following are the EQE curves of organic solar cell devices based on PBDB-T:YO4Cl-Dq, PBDB-T:YO4Cl-BO and PBDB-T:YO4Cl-Se. It can be found that the three devices have good light response in the spectral range of 300-710nm. Among them, the EQE of the PBDB-T:YO4Cl-Dq device in the range of 400-670nm exceeds 70%, while the responsiveness of PBDB-T:YO4Cl-BO and PBDB-T:YO4Cl-Se in this range is higher, with a responsivity of more than 75%. Therefore, the three devices show excellent performance.
[0125] Fig.10 The J–V characteristic curves of the stacked cells prepared with PM6:Y6-BO / Y6-O / BTP-S3 and PBDB-T:YO4Cl-Se as the front cell and PTTzF:Y6:
[70] PCBM as the back cell were obtained. The PM6:Y6-BO device exhibited an open circuit voltage of 1.68 V, a short circuit current of 14.50 mA / cm2, and a fill factor of 77.21%. Finally, an efficiency of 18.81% was achieved. The PM6:Y6-O device exhibited an open circuit voltage of 1.75 V, a short circuit current of 14.30 mA / cm2, and a fill factor of 77.25%. Finally, an efficiency of 19.33% was achieved. The PM6:BTP-S3 device exhibited an open circuit voltage of 1.92 V, a short circuit current of 13.75 mA / cm2, and a fill factor of 65.34%. Finally, an efficiency of 17.25% was achieved. The PBDB-T:YO4Cl-Se device exhibited an open-circuit voltage of 1.91 V and a short-circuit current of 14.37 mA / cm2 with a fill factor of 75.22%. The final efficiency was 20.65%.
[0126] Fig.11The J–V characteristic curves of single-junction cells with PM6:Y6-BO / Y6-O / BTP-S3 and PBDB-T:YO4Cl-Se as active layers under indoor lighting conditions are shown. The PM6:Y6-BO device exhibits an open circuit voltage of 0.71 V, a short circuit current of 119.69 μA / cm2, and a fill factor of 75.46%. Finally, an efficiency of 22.58% was achieved. The PM6:Y6-O device exhibits an open circuit voltage of 0.86 V, a short circuit current of 126.32 μA / cm2, and a fill factor of 80.02%. Finally, an efficiency of 30.61% was achieved. The PM6:BTP-S3 device exhibits an open circuit voltage of 0.92 V, a short circuit current of 114.24 μA / cm2, and a fill factor of 53.69%. Finally, an efficiency of 19.87% was achieved. The PBDB-T:YO4Cl-Se device exhibited an open-circuit voltage of 0.94 V and a short-circuit current of 120.43 μA / cm2 with a fill factor of 78.35%. The final efficiency was 31.23%.
[0127] Embodiment 11
[0128] The materials obtained in the examples (YO4Cl-Dq, YO4Cl-BO, YO4Cl-Se) are used as examples to illustrate the application of the medium bandgap acceptor materials of the present invention in organic solar cells and indoor photovoltaic devices, but the present invention is not limited to the examples given.
[0129] The specific preparation process of the device is as follows:
[0130] (1) Single junction device preparation
[0131] A 40nm hole transport layer (PEDOT:PSS) was spin-coated on the ITO glass, followed by a 100nm photoactive layer of the donor and acceptor materials, and then a 5nm PFN-Br layer was spin-coated as the cathode interface layer, and then a 100nm Ag electrode was evaporated to complete the device preparation. The device was then tested under a standard solar simulator and an indoor light simulator.
[0132] (2) Preparation of stacked devices
[0133] The stacked device adopts the following structure: ITO / PEDOT:PSS / front cell active layer / connection layer / rear cell active layer / PDINO / Ag. The preparation process of the front cell active layer is the same as that of the single-cell device. Preparation of the connection layer (ZnO / PEDOT:PSS / PMA): First, a ZnO nanoparticle layer (about 20nm) is spin-coated on the active layer of the front cell, and then PEDOT:PSS (diluted with deionized water at a ratio of 1:2.5) is spin-coated on the ZnO layer (about 15nm). The substrate is thermally annealed at 100℃ for 5min, and then about 5nm of phosphomolybdic acid (PMA) is spin-coated on PEDOT:PSS. The preparation method of the rear cell active layer is the same as that of the single-cell device. After the front cell, connection layer and rear cell active layer are prepared, the electron transport layer PDINO is spin-coated (3000rpm). Finally, the Ag electrode is deposited by evaporation under high vacuum to obtain a stacked cell device.
[0134] Table 1. Performance parameters of device ITO / PEDOT:PSS / PBDB-T:Acceptor / PFN-Br / Ag (AM1.5G)
[0135]
[0136] Table 2. Performance parameters of stacked solar cells prepared with ITO / PEDOT:PSS / PBDB-T:acceptor / PFN-Br / Ag as the front cell and ITO / PEDOT:PSS / PTTzF:Y6:
[70] PCBM / PDINO / Ag as the back cell (AM1.5G)
[0137]
[0138] Table 3. Performance parameters of tandem solar cells obtained by using ITO / PEDOT:PSS / PBDB-T:YO4Cl-Se / PFN-Br / Ag as the front cell, PTTzF:Y6:
[70] PCBM, PTB7-Th:O6T-4F and PM6:BTP-eC9 as the active layer, and the device structure is ITO / PEDOT:PSS / active layer / PDINO / Ag as the back cell (AM1.5G)
[0139]
[0140] Table 4. Performance parameters of ITO / PEDOT:PSS / PBDB-T:Acceptor / PFN-Br / Ag devices under indoor lighting (1000 Lux, input power (P in ) is 284 microwatts per square centimeter)
[0141]
[0142] As shown in Table 1, the single junction devices prepared with PBDB-T as donor and YO4Cl-Dq, YO4Cl-BO and YO4Cl-Se as acceptors all exhibited an open circuit voltage of more than 1.1 V, a high fill factor and good device efficiency. The corresponding JV curves and EQE curves are shown in the attached Figure 8 and 9 , which shows that this type of material has great application potential. The front cells were prepared with PBDB-T:YO4Cl-Dq, PBDB-T:YO4Cl-BO and PBDB-T:YO4Cl-Se as the active layer, and the back cells were prepared with PTTzF:Y6:
[70] PCBM as the active layer. The performance of the tandem solar cell device is shown in Table 2. Due to the good complementary absorption of the medium bandgap material and the narrow bandgap material, as well as the excellent open circuit voltage and photovoltaic performance of the front cell, the efficiency of the above-mentioned tandem solar cell devices exceeds 20%. In particular, the efficiency of the tandem cell device based on YO4Cl-Se reached 20.65%. In addition, in order to study the universality of medium bandgap materials in tandem cells, the front cell with PBDB-T:YO4Cl-Se as the active layer was matched with different back cells, and the device data are shown in Table 3. It can be found that the precell based on the medium-bandgap acceptor not only matches well with PTTzF:Y6:
[70] PCBM, but also achieves 19.87% and 20.45% efficiency in the stacked device with PTB7-Th:O6T-4F and PM6:BTP-eC9, respectively. The above results show that the medium-bandgap acceptor material in the present invention not only exhibits good device efficiency in single-junction devices, but also has excellent performance and universality in stacked cell devices, and is a class of precell materials with great potential.
[0143] The single junction devices based on YO4Cl-Dq, YO4Cl-BO and YO4Cl-Se have absorption spectra that are very compatible with the luminescence spectra of indoor light sources. The device performance obtained by placing the single junction devices of PBDB-T:YO4Cl-Dq, YO4Cl-BO or YO4Cl-Se under indoor lighting conditions is shown in Table 4. The devices based on YO4Cl-Dq, YO4Cl-BO and YO4Cl-Se showed excellent device efficiencies of 31.04%, 30.41% and 31.23%, respectively. This result shows that the medium bandgap acceptor in the present invention has good application in the field of indoor photovoltaics.
[0144] Comparative Example
[0145]
[0146] In order to further illustrate that the medium band gap receptors involved in the present invention have unique advantages in OSCs, taking the embodiment YO4Cl-Se involved in the present invention as an example, similar and representative receptors are selected for comparison (Comparative Examples 1-3). Among them, the Y6-BO molecule is modified with an alkyl side chain and a condensed ring structure and is matched with a strong electron-withdrawing end group (Comparative Example 1); the Y6-O molecule is modified with an alkoxy side chain and a strong electron-withdrawing unit is used as an end group (Comparative Example 2); and the BTP-S3 molecule uses a condensed ring structure modified with a weak electron-withdrawing end group and an alkyl side chain (Comparative Example 3). Under the same conditions, single-junction devices and stacked devices were prepared using the above four materials as receptors, and the single-junction devices were tested under standard sunlight and indoor light environments, respectively. The relevant device data are shown in Tables 5-7.
[0147] Table 5. Device parameters of single-junction organic solar cells based on PM6:Y6-BO / Y6-O / BTP-S3 and PBDB-T:YO4Cl-Se under standard sunlight conditions (AM1.5G)
[0148]
[0149] From the single junction device data (Table 5), it can be found that compared with Comparative Examples 1 and 2, the open circuit voltage of the PBDB-T:YO4Cl-Se device is significantly increased due to the higher LUMO energy level of YO4Cl-Se. Compared with Comparative Example 3, the fill factor of the PBDB-T:YO4Cl-Se device is significantly higher than that of the PM6:BTP-S3 device due to its excellent morphology. Finally, the PBDB-T:YO4Cl-Se-based device exhibits high open circuit voltage and good device performance.
[0150] Table 6. Device parameters of tandem organic solar cells prepared with PM6:Y6-BO / Y6-O / BTP-S3 and PBDB-T:YO4Cl-Se as front cells and PTTzF:Y6:
[70] PCBM as back cells under standard sunlight conditions (AM1.5G)
[0151]
[0152] Front cells were prepared using YO4Cl-Se and three comparative materials as acceptors, and rear cells were prepared using PTTzF:Y6:
[70] PCBM as active layers to obtain stacked solar cell devices. The device performance is shown in Table 6. Since the single-junction device of PBDB-T:YO4Cl-Se has a higher open circuit voltage than the devices of Comparative Example 1 and Comparative Example 2, the open circuit voltage of the stacked device based on PBDB-T:YO4Cl-Se is significantly higher than the former two. Similarly, since the fill factor of the device of Comparative Example 3 is low, the efficiency of the stacked device is only 17.25%. Thanks to the high open circuit voltage and excellent device performance of the PBDB-T:YO4Cl-Se device, the stacked device based on PBDB-T:YO4Cl-Se achieved a device efficiency of 20.65%, which is higher than all comparative examples. This further illustrates that the medium bandgap acceptor reported in the present invention is a good front cell material.
[0153] Table 7. Device parameters of PM6:Y6-BO / Y6-O / BTP-S3 and PBDB-T:YO4Cl-Se single junction devices under indoor light conditions (1000Lux, input power (P in ) is 284 microwatts per square centimeter)
[0154]
[0155] The device performance of single-junction devices based on the above four acceptor materials under indoor lighting conditions is shown in Table 7. Due to the blue shift of the spectrum of YO4Cl-Se and its high LUMO energy level, the device based on PBDB-T:YO4Cl-Se exhibits a higher open circuit voltage than Comparative Example 1 and Comparative Example 2. Not only that, since the PBDB-T:YO4Cl-Se active layer has a good device morphology, the filling factor is greatly improved compared to Comparative Example 3. In summary, the device based on PBDB-T:YO4Cl-Se achieved an optimal device efficiency of 31.23% under indoor lighting. The above results show that the medium bandgap acceptor in the present invention is more suitable for indoor photovoltaic devices than the comparative example materials.
[0156] In summary, the medium-bandgap fused ring acceptor molecules obtained by using alkoxy side chain thiophene structure and weak electron-withdrawing end group have high absorption coefficient and high LUMO energy level. When such materials are used in OSCs, they can significantly improve the open circuit voltage while obtaining excellent device performance. In addition, the application of such materials in tandem solar cells and indoor photovoltaics has achieved a breakthrough in the efficiency of tandem solar cells and indoor photovoltaic devices.
[0157] The above embodiments of the present invention are only examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A medium band gap fused ring receptor material, the general structure of which is shown in Formula I: in: In the structural formula, R1 and R2 are independently selected from a linear, branched or alkyl-substituted aromatic chain having 1 to 40 carbon atoms; The Weak A unit is a weak electron withdrawing group, selected from any one of the following structural formulas: in: The dotted line in the Weak A structure indicates the connection site to the Weak A unit.
2. A medium band gap fused ring receptor material according to claim 1, characterized in that: The Ar1 unit is selected from any one of the following structural formulas: Wherein, R3 in the Ar1 structural formula is independently selected from H, a linear, branched or alkyl-substituted aromatic chain having 1 to 20 carbon atoms, and the dotted line in the Ar1 structural formula represents the connection site with other units.
3. A method for preparing a medium band gap fused ring receptor material according to claim 1 or 2, comprising the following steps: Its synthetic route is as follows: In the structural formula, R1 and R2 are independently selected from a linear, branched or alkyl-substituted aromatic chain having 1 to 40 carbon atoms.
4. The preparation method according to claim 3, characterized in that: The steps include: (1) Compound A and Compound B are added to 80-100 mL of toluene, and a catalyst of tris(dibenzylideneacetone)dipalladium and tris(o-methylphenyl)phosphine is added to obtain Compound C through Stille coupling reaction; (2) Under nitrogen protection, compound C and triphenylphosphine are added to o-dichlorobenzene and heated to react to obtain compound D; (3) Under nitrogen protection, compound D, halogenated alkane (R2-Br), potassium carbonate and potassium iodide are added to N,N-dimethylformamide to react to obtain compound E; (4) This reaction is a Vilsmeier-Haack reaction. Under nitrogen protection, compound E is dissolved in 1,2-dichloroethane, and then added dropwise to the formylation reagent phosphorus oxychloride at -10 to 0°C; after reacting at -10 to 0°C for 1 to 2 hours, the system is heated to 80 to 100°C and reacted for 8 to 12 hours to obtain compound F; (5) This reaction is a Knoevenagel condensation reaction. Under nitrogen protection, compound F is reacted with pyridine to obtain compound G.
5. The preparation method according to claim 4, characterized in that: In step (1), the conditions for the Stille coupling reaction are: reaction at 80-85° C. for 4-6 hours.
6. The preparation method according to claim 4, characterized in that: In step (2), the heating reaction is specifically heating to 160-180° C. for 15-18 hours.
7. The preparation method according to claim 4, characterized in that: In step (3), the reaction is carried out at 80-85° C. for 10-12 hours.
8. The preparation method according to claim 4, characterized in that: In step (4), the molar ratio of compound E to phosphorus oxychloride is 1:10 to 1:
30.
9. The preparation method according to claim 4, characterized in that: In step (5), the reaction is carried out at 60-65° C. for 5-8 hours.
10. The medium band gap fused ring acceptor material according to claim 1 or 2 is used in photovoltaic devices.
Citation Information
Patent Citations
N-type organic semiconductor material as well as preparation method and application thereof
CN112375212A
Novel synthesis method of A-D-A type organic semiconductor material
CN115785118A
Preparation method of compound containing thiophene structure, obtained compound and application
CN115873015A
Condensed ring organic compound and application thereof in organic electronic device
CN115873024A
Dibenzo quinoxaline wide-band-gap acceptor material for organic solar cell and preparation method and application of dibenzo quinoxaline wide-band-gap acceptor material
CN116514836A
Cited By
Alkoxy-substituted organic compound and application thereof
CN119350370A
Phenolazine derivative ultra-narrow band gap receptor, preparation method thereof and application of phenolazine derivative ultra-narrow band gap receptor in organic solar cell
CN119912474A
A phenoxazine derivative ultra-narrow band gap acceptor, a preparation method thereof and use thereof in organic solar cells
CN119912474B
Electron acceptor containing sulfur bridging central unit as well as preparation method and application of electron acceptor
CN120098004A