Antioxidant polyvinyl alcohol derivative containing 1, 4-dihydropyridine structure as well as preparation method and application of antioxidant polyvinyl alcohol derivative

By modifying and modifying polyvinyl alcohol and introducing 1,4-dihydropyridine structure, the problem that polyvinyl alcohol itself does not have antioxidant properties is solved, significantly improves the antioxidant ability and stability, and is suitable for multiple fields. Materials application.

CN119019596AActive Publication Date: 2024-11-26CHINA PETROLEUM & CHEMICAL CORP +2
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310602945.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-11-26
Estimated Expiration
2043-05-25

AI Technical Summary

Technical Problem

Polyvinyl alcohol itself does not have antioxidant properties. The existing method of blending small molecule antioxidants into the material has problems such as poor stability, fast migration, and affecting the processing performance of the material, which limits its development in the fields of biomedical, packaging, and health care. .

Method used

By modifying and modifying polyvinyl alcohol, 1,4-dihydropyridine structure was introduced, and antioxidant polyvinyl alcohol derivatives were prepared under mild reaction conditions by one pot method to improve the stability and safety of their antioxidant groups. , prolong metabolism or migration time.

Benefits of technology

It significantly improves the antioxidant ability of polyvinyl alcohol and the utilization of materials, maintains the solvent resistance and film formation of polyvinyl alcohol itself, and is suitable for biomedical, packaging, health care and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019596A_ABST
    Figure CN119019596A_ABST
Patent Text Reader

Abstract

The invention provides an antioxidant polyvinyl alcohol derivative containing a 1, 4-dihydropyridine structure as well as a preparation method and application of the antioxidant polyvinyl alcohol derivative. The antioxidant polyvinyl alcohol derivative comprises a structural unit containing 1, 4-dihydropyridine, a vinyl alcohol structural unit and a vinyl acetate structural unit. The preparation method comprises the following steps: dissolving polyvinyl alcohol in an anhydrous organic solvent, adding diketene for reaction to obtain a beta-diketone-containing polyvinyl alcohol derivative, in the presence of a catalyst, adding an aldehyde compound, an ammonia source compound and a 1, 3-diketone compound into the beta-diketone-containing polyvinyl alcohol derivative for Hantzsch reaction to obtain the beta-diketone-containing polyvinyl alcohol derivative. The antioxidant polyvinyl alcohol derivative containing the 1, 4-dihydropyridine structure is obtained. The prepared polyvinyl alcohol derivative has excellent oxidation resistance and can be applied to the fields of food packaging, biological medicine, health care and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of functional polymer materials, and more particularly to an antioxidant polyvinyl alcohol derivative containing a 1,4-dihydropyridine structure, and a preparation method and application thereof. Background Art

[0002] Polyvinyl alcohol (PVA) is a hydrophilic, environmentally friendly vinyl polymer, generally prepared on a large scale industrially by hydrolysis of polyvinyl acetate. It is inexpensive, biodegradable, and has good solvent resistance, film-forming properties, low protein adsorption, biocompatibility, and biodegradability. It can be used as food packaging, contact lenses, vascular embolization particles, artificial pancreas, artificial cartilage, meniscus and other products, and has a wide range of applications in the food packaging industry and biomedical fields.

[0003] In the field of active food packaging and the treatment of diseases related to oxidative stress (such as neurodegenerative diseases, cardiovascular diseases, eye diseases, wound repair, etc.), materials with antioxidant properties have attracted much attention. Polyvinyl alcohol is often compounded with other antioxidant components to form functional antioxidant materials, such as combined with antioxidant components such as natural polyphenols to prepare antioxidant hydrogels, PVA-based active packaging materials, etc. However, polyvinyl alcohol itself does not have antioxidant properties and must be modified by adding active substances. For example, Sun Miao and Deng Jing, etc. prepared inclusion complexes embedded in β-cyclodextrin of clove essential oil and blended them with PVA to form films; Zhang Yan, etc. modified PVA films with different contents of citric acid, etc. However, these methods of blending small molecule antioxidants into PVA materials have problems such as poor stability, fast migration, and influence on material processing performance. They are easy to migrate and dissolve during use, and have poor durability, which to a certain extent limits their development as biomedical, packaging, and health care materials. Therefore, it is of great significance to modify polyvinyl alcohol so that it can produce antioxidant capacity itself, which can significantly improve the stability and safety of antioxidant groups, prolong metabolism or migration time, and improve the utilization of materials. Summary of the invention

[0004] In order to solve the technical problems existing in the prior art, the present invention provides an antioxidant polyvinyl alcohol derivative containing a 1,4-dihydropyridine structure, and a preparation method and application thereof.

[0005] The present invention can prepare antioxidant polyvinyl alcohol derivatives containing 1,4-dihydropyridine structure in large quantities, simply and efficiently. The present invention uses commercially available polyvinyl alcohol, which is widely available, cheap and easily available, as the main raw material, obtains polyvinyl alcohol derivatives with excellent antioxidant properties in high yield through a simple preparation reaction process under mild reaction conditions, and confirms its antioxidant applicability.

[0006] The present invention modifies polyvinyl alcohol so that it can produce antioxidant capacity, which can significantly improve the stability and safety of antioxidant groups, prolong metabolism or migration time, and improve the utilization of materials. At the same time, the polyvinyl alcohol unit can be retained on the main chain, and the properties of polyvinyl alcohol itself, such as good solvent resistance and film-forming properties, can be prepared as an antioxidant film material.

[0007] The polyvinyl alcohol derivatives prepared by the present invention can change various properties such as antioxidant property, water solubility, solvent resistance and film-forming property of the derivatives by adjusting the proportion of 1,4-dihydropyridine structural units, and can be applied to various fields such as biomedicine, packaging, and health care materials.

[0008] In the prior art, post-modification of polyvinyl alcohol generally requires purification of intermediate products, while the preparation method of polyvinyl alcohol derivatives (i.e., post-modification of polyvinyl alcohol) of the present invention adopts a one-pot method, which does not require purification of intermediate products, has mild reaction conditions, and is simple in preparation method, and can obtain polyvinyl alcohol derivatives with excellent antioxidant properties in high yield.

[0009] One of the purposes of the present invention is to provide an antioxidant polyvinyl alcohol derivative containing a 1,4-dihydropyridine structure.

[0010] The antioxidant polyvinyl alcohol derivative comprises a structural unit containing 1,4-dihydropyridine, a vinyl alcohol structural unit and a vinyl acetate structural unit;

[0011] The structural unit containing 1,4-dihydropyridine is of formula I:

[0012]

[0013] The vinyl alcohol structural unit is of formula II:

[0014]

[0015] The vinyl acetate structural unit is of formula III:

[0016]

[0017] In formula I, R is phenyl, substituted phenyl, heterocyclic aromatic group or C1-C8 alkyl group, the substituted phenyl group is preferably 3-methoxy-4-hydroxyphenyl, p-hydroxyphenyl or 3,4-dihydroxyphenyl, and the heterocyclic aromatic group is preferably 2-thienyl;

[0018] The molar percentages of the structural units containing 1,4-dihydropyridine, the vinyl alcohol structural units and the vinyl acetate structural units are x, y and z respectively, and x+y+z=1; wherein x+y=alcoholysis degree, and the alcoholysis degree is 88-99%; preferably, x is 4-99mol%, y is 0-95mol%, and the rest is z; further preferably, x is 4-91mol%, y is 8-95mol%, and the rest is z; further preferably, x is 4-60mol%, y is 25-95mol%, and the rest is z.

[0019] Polyvinyl alcohol is obtained by alcoholysis of polyvinyl acetate. The alcoholysis degree refers to the percentage of vinyl alcohol units in the molecular chain to the total number of molecular structural units. The molar percentages of the structural units of formula I and formula II satisfy that the sum of the two is equal to the alcoholysis degree.

[0020] The second object of the present invention is to provide a method for preparing an antioxidant polyvinyl alcohol derivative containing a 1,4-dihydropyridine structure, comprising the following steps:

[0021] (1) dissolving polyvinyl alcohol in an anhydrous organic solvent, adding diketene to react to obtain a polyvinyl alcohol derivative containing β-diketone;

[0022] (2) In the presence of a catalyst, an aldehyde compound, an ammonia source compound and a 1,3-diketone compound are added to the polyvinyl alcohol derivative containing β-diketone obtained in step (1) to carry out a Hantzsch reaction to obtain the antioxidant polyvinyl alcohol derivative containing a 1,4-dihydropyridine structure.

[0023] In a preferred embodiment of the present invention,

[0024] Step (1),

[0025] The polyvinyl alcohol has a polymerization degree of 500-1700 and an alcoholysis degree of 88-99%; preferably at least one of PVA1788, PVA1799 and PVA0588;

[0026] The anhydrous organic solvent is preferably at least one of anhydrous N-methylpyrrolidone (NMP), anhydrous dimethyl sulfoxide (DMSO), and anhydrous N,N-dimethylformamide (DMF); anhydrous means that the water content is extremely low, and the water content is usually required to be less than or equal to 50 ppm.

[0027] In a preferred embodiment of the present invention,

[0028] Step (1),

[0029] The mass of the polyvinyl alcohol and the volume of the solvent are 0.05 to 0.3 g / ml, preferably 0.08 to 0.2 g / ml;

[0030] The molar ratio of the hydroxyl group in the polyvinyl alcohol to the diketene is 1:(0.01-1), preferably 1:(0.1-0.9);

[0031] The reaction temperature is 25 to 40°C, preferably 25 to 35°C;

[0032] The reaction time is 1 to 3 hours, preferably 1 to 2 hours.

[0033] In a preferred embodiment of the present invention,

[0034] Step (2),

[0035] The catalyst is an amino acid catalyst or other weakly acidic catalyst, preferably glycine, proline or phenylboronic acid;

[0036] The aldehyde compound is preferably at least one of benzaldehyde, substituted benzaldehyde, heterocyclic aromatic aldehyde, and C1-C8 fatty aldehydes; the substituted benzaldehyde is preferably at least one of vanillin, p-hydroxybenzaldehyde, and 3,4-dihydroxybenzaldehyde; the heterocyclic aromatic aldehyde is preferably 2-thiophenecarboxaldehyde;

[0037] The ammonia source compound is preferably at least one of ammonium acetate, ammonium carbonate, and ammonia water;

[0038] The 1,3-diketone compound is at least one of 1,3-cyclohexanedione and its derivatives, preferably at least one of 1,3-cyclohexanedione, 5-methyl-1,3-cyclohexanedione and 5,5-dimethyl-1,3-cyclohexanedione.

[0039] In a preferred embodiment of the present invention,

[0040] Step (2),

[0041] The conditions of the Hantzsch reaction are as follows:

[0042] The molar ratio of the aldehyde compound, the ammonia source compound and the 1,3-diketone compound is 1:(1-2):(1-1.2), preferably 1:(1.2-1.6):(1-1.2), more preferably 1:(1.2-1.6):1;

[0043] The molar ratio of the aldehyde compound to diketene is (1-2):1, preferably (1.1-1.5):1;

[0044] The molar ratio of the catalyst to the aldehyde compound is (0.05-0.2):1, preferably (0.1-0.15):1;

[0045] The reaction temperature is 70 to 90°C, preferably 70 to 80°C;

[0046] The reaction time is 2 to 5 hours, preferably 2 to 4 hours.

[0047] In a preferred embodiment of the present invention,

[0048] After the polyvinyl alcohol derivative containing β-diketone is obtained in step (1), it can be directly subjected to step (2) for Hantzsch reaction without purification;

[0049] Step (2) After the Hantzsch reaction is completed, the polyvinyl alcohol derivative containing a 1,4-dihydropyridine structure is collected by an organic solvent precipitation method, that is, after the Hantzsch reaction is completed, the reaction solution is poured into an organic solvent, and the precipitate is collected to obtain the polyvinyl alcohol derivative containing a 1,4-dihydropyridine structure.

[0050] In a preferred embodiment of the present invention,

[0051] The organic solvent is a commonly used organic solvent in the prior art, preferably at least one of methanol, ethanol, acetone and acetonitrile.

[0052] The third object of the present invention is to provide an antioxidant polyvinyl alcohol derivative containing a 1,4-dihydropyridine structure obtained by the above preparation method.

[0053] By using the above preparation method, an antioxidant 1,4-dihydropyridine structure is introduced into the side chain of polyvinyl alcohol, and the modified polyvinyl alcohol derivative thus obtained also has significant antioxidant ability.

[0054] A fourth object of the present invention is to provide an application of an antioxidant polyvinyl alcohol derivative containing a 1,4-dihydropyridine structure, such as its application in the fields of medicine, health and food packaging.

[0055] The endpoints and any values ​​of the scope disclosed in the present invention are not limited to the precise scope or value, and these scopes or values ​​should be understood to include values ​​close to these scopes or values. For numerical ranges, the endpoint values ​​of each scope, the endpoint values ​​of each scope and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in this article. Hereinafter, in principle, each technical solution can be combined with each other to obtain a new technical solution, which should also be regarded as specifically disclosed in this article.

[0056] Compared with the prior art, the present invention has at least the following advantages:

[0057] The invention adopts a one-pot method to prepare antioxidant polyvinyl alcohol derivatives containing 1,4-dihydropyridine structure in large quantities, simply and efficiently; the invention uses commercially available polyvinyl alcohol as a main raw material, which has a wide source, is cheap and easy to obtain, has a simple preparation process, a high yield and mild reaction conditions; the prepared polyvinyl alcohol derivatives have excellent antioxidant properties and have great application potential in the fields of food packaging, biomedicine, health care and the like. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1 The synthetic route of the antioxidant polyvinyl alcohol derivative containing 1,4-dihydropyridine structure in the present invention;

[0059] Figure 2 The hydrogen nuclear magnetic spectrum of the antioxidant polyvinyl alcohol derivative (P1) containing 1,4-dihydropyridine structure synthesized in Example 1 ( 1 H-NMR);

[0060] Figure 3 The hydrogen nuclear magnetic spectrum of the antioxidant polyvinyl alcohol derivative (P2) containing 1,4-dihydropyridine structure synthesized in Example 2 ( 1 H-NMR);

[0061] Figure 4 The hydrogen nuclear magnetic spectrum of the antioxidant polyvinyl alcohol derivative (P3) containing 1,4-dihydropyridine structure synthesized in Example 3 ( 1 H-NMR);

[0062] Figure 5 The hydrogen nuclear magnetic spectrum of the antioxidant polyvinyl alcohol derivative (P4) containing 1,4-dihydropyridine structure synthesized in Example 4 ( 1 H-NMR);

[0063] Figure 6 The hydrogen nuclear magnetic spectrum of the antioxidant polyvinyl alcohol derivative (P1′) containing a 1,4-dihydropyridine structure synthesized in Example 5 ( 1 H-NMR);

[0064] Figure 7 The hydrogen nuclear magnetic spectrum of the antioxidant polyvinyl alcohol derivative (P4′) containing a 1,4-dihydropyridine structure synthesized in Example 6 ( 1 H-NMR);

[0065] Figure 8 ABTS of P1, P2, P3, and P4 in Examples 1 to 4 +· Quenching kinetics curve. DETAILED DESCRIPTION

[0066] The present invention is described in detail below in conjunction with specific drawings and embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the content of the present invention still fall within the scope of protection of the present invention.

[0067] It should also be noted that the various specific technical features described in the following specific embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0068] In addition, the various embodiments of the present invention may be arbitrarily combined as long as they do not violate the concept of the present invention. The technical solutions thus formed belong to part of the original disclosure of this specification and also fall within the protection scope of the present invention.

[0069] Test method:

[0070] a Free radical quenching ability test method: Mix the aqueous solution of 2,2'-azobis-3-ethylbenzothiazoline-6-sulfonic acid diammonium salt and the aqueous solution of potassium persulfate and place them in the dark for 14 hours to obtain ABTS +· ABTS +· The stock solution was diluted with PBS buffer to an absorbance of about 0.7 to obtain ABTS +· Working solution. Prepare 2 mg / mL P1-P4 polymer solution with PBS buffer. Mix the polymer solution and ABTS +· The working solutions were mixed in equal proportions, and the absorbance change of the solution at 734 nm was detected by an enzyme-labeled instrument.

[0071] The references for this method are as follows:

[0072] 1. Jeddou, KB; Chaari, F.; Maktouf, S.; Nouri-Ellouz, O.; Helbert, CB; Ghorbel, RE, Structural, functional, and antioxidant properties of water-soluble polysaccharides from potatoes peels. Food Chem. 2016, 205, 97-105.

[0073] 2.Mao, T.; Yang, L.; Liu, G.; Wei, Y.; Gou, Y.; Wang, J.; Tao, L., Ferrocene-Containing Polymer via the Biginelli Reaction for In Vivo Treatment of Oxidative Stress Damage. ACS Macro Lett. 2019, 8(6), 639-645.

[0074] b. Testing method for the molar percentage of each structural unit: In the present invention, the method can be 1 H NMR confirmed the structure of PVA after antioxidant modification and the proportion of each structural unit.

[0075] The present invention will be described in detail below through examples.

[0076] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.

[0077] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0078] Some raw material specifications:

[0079] Polyvinyl alcohol 0588, degree of polymerization 500, degree of alcoholysis 88%;

[0080] Polyvinyl alcohol 1788, degree of polymerization 1700, degree of alcoholysis 88%;

[0081] Polyvinyl alcohol 1799, degree of polymerization 1700, alcoholysis degree 99%;

[0082] The above polyvinyl alcohols were all purchased from Anhui Wanwei Group Co., Ltd.

[0083] Example 1

[0084] The reaction equation is Figure 1 shown.

[0085] Dissolve polyvinyl alcohol 0588 (1.1 g, hydroxyl molar amount about 22 mmol) in anhydrous N-methylpyrrolidone (10 mL) to form a clear transparent solution, add diketene (184.9 mg, 2.2 mmol), and stir at 25°C for 1 hour. Then add benzaldehyde (256.8 mg, 2.42 mmol), 5,5-dimethyl-1,3-cyclohexanedione (339.2 mg, 2.42 mmol), ammonium acetate (279.8 mg, 3.63 mmol), and glycine (18.2 mg, 0.24 mmol) to the reaction liquid system, and heat the reaction liquid system to 80°C for 3.5 hours. After the reaction is completed, the reaction liquid is precipitated in an acetone solution to obtain 1.5 g of polyvinyl alcohol derivative P1 containing a 1,4-dihydropyridine structure.

[0086] P1 contains the following structural units:

[0087]

[0088] Wherein R is a benzaldehyde side chain group, x is 0.07, y is 0.81, and z is 0.12.

[0089] Depend on Figure 2 Shown 1 From the H-NMR spectrum, it can be seen that the characteristic peak of the benzene ring appears at the chemical shift of 6.95-7.15ppm, and the characteristic peak of nitrogen and hydrogen on the dihydropyridine ring appears at about 8.97ppm. It can be seen that the target polyvinyl alcohol derivative P1 containing a 1,4-dihydropyridine structure is obtained in this example.

[0090] Example 2

[0091] The reaction equation is Figure 1 shown.

[0092] Dissolve polyvinyl alcohol 0588 (1.1 g, hydroxyl molar amount about 22 mmol) in anhydrous N-methylpyrrolidone (10 mL) to form a clear transparent solution, add diethyl ketone (184.9 mg, 2.2 mmol), and stir at 25 ° C for 1 hour. Then add vanillin (368.2 mg, 2.42 mmol), 5,5-dimethyl-1,3-cyclohexanedione (339.2 mg, 2.42 mmol), ammonium acetate (279.8 mg, 3.63 mmol), and glycine (18.2 mg, 0.24 mmol) to the reaction liquid system, and heat the reaction liquid system to 80 ° C for 3.5 hours. After the reaction is completed, the reaction liquid is precipitated in an acetone solution to obtain 1.6 g of polyvinyl alcohol derivative P2 containing a 1,4-dihydropyridine structure.

[0093] P2 contains the following structural units:

[0094]

[0095] Wherein R is the vanillin side chain group, x is 0.07, y is 0.81, and z is 0.12.

[0096] Depend on Figure 3 Shown 1 From the H-NMR spectrum, it can be seen that the characteristic peak of the benzene ring appears at the chemical shift of 6.43-6.67ppm, and the characteristic peak of nitrogen and hydrogen on the dihydropyridine ring appears at about 8.92ppm. It can be seen that the target polyvinyl alcohol derivative P2 containing a 1,4-dihydropyridine structure is obtained in this example.

[0097] Example 3

[0098] The reaction equation is Figure 1 shown.

[0099] Dissolve polyvinyl alcohol 0588 (1.1 g, hydroxyl molar amount about 22 mmol) in anhydrous N-methylpyrrolidone (10 mL) to form a clear transparent solution, add diketene (184.9 mg, 2.2 mmol), and stir at 25 ° C for 1 hour. Then add p-hydroxybenzaldehyde (295.5 mg, 2.42 mmol), 5,5-dimethyl-1,3-cyclohexanedione (339.2 mg, 2.42 mmol), ammonium acetate (279.8 mg, 3.63 mmol), and glycine (18.2 mg, 0.24 mmol) to the reaction liquid system, and heat the reaction liquid system to 80 ° C for 3.5 hours. After the reaction is completed, the reaction liquid is precipitated in an acetone solution to obtain 1.5 g of polyvinyl alcohol derivative P3 containing a 1,4-dihydropyridine structure.

[0100] P3 contains the following structural units:

[0101]

[0102] Wherein R is the side chain group of p-hydroxybenzaldehyde, x is 0.04, y is 0.84, and z is 0.12.

[0103] Depend on Figure 4 Shown 1 From the H-NMR spectrum, it can be seen that the characteristic peak of the benzene ring appears at the chemical shift of 6.45-6.93ppm, and the characteristic peak of nitrogen and hydrogen on the dihydropyridine ring appears at about 8.90ppm. It can be seen that the target polyvinyl alcohol derivative P3 containing a 1,4-dihydropyridine structure is obtained in this example.

[0104] Example 4

[0105] The reaction equation is Figure 1 shown.

[0106] Dissolve polyvinyl alcohol 0588 (1.1 g, hydroxyl molar amount about 22 mmol) in anhydrous N-methylpyrrolidone (10 mL) to form a clear transparent solution, add diketene (184.9 mg, 2.2 mmol), and stir at 25 ° C for 1 hour. Then add 3,4-dihydroxybenzaldehyde (334.3 mg, 2.42 mmol), 5,5-dimethyl-1,3-cyclohexanedione (339.2 mg, 2.42 mmol), ammonium acetate (279.8 mg, 3.63 mmol), and glycine (18.2 mg, 0.24 mmol) to the reaction liquid system, and heat the reaction liquid system to 80 ° C for 3.5 hours. After the reaction is completed, the reaction liquid is precipitated in an acetone solution to obtain 1.6 g of polyvinyl alcohol derivative P4 containing a 1,4-dihydropyridine structure.

[0107] P4 contains the following structural units:

[0108]

[0109] Wherein R is a side chain group of 3,4-dihydroxybenzaldehyde, x is 0.04, y is 0.84, and z is 0.12.

[0110] Depend on Figure 5 Shown 1 From the H-NMR spectrum, it can be seen that the characteristic peak of the benzene ring appears at the chemical shift of 6.30-6.55 ppm, and the characteristic peak of nitrogen and hydrogen on the dihydropyridine ring appears at about 8.87 ppm. It can be seen that the target polyvinyl alcohol derivative P4 containing a 1,4-dihydropyridine structure is obtained in this example.

[0111] Example 5

[0112] The reaction equation is Figure 1 shown.

[0113] Dissolve polyvinyl alcohol 0588 (1.1 g, hydroxyl molar amount about 22 mmol) in anhydrous N-methylpyrrolidone (10 mL) to form a clear transparent solution, add diketene (1.66 g, 19.8 mmol), and stir at 35 ° C for 2 hours. Then add benzaldehyde (2.31 g, 21.78 mmol), 5,5-dimethyl-1,3-cyclohexanedione (3.66 g, 26.14 mmol), ammonium acetate (2.02 g, 26.14 mmol), and glycine (163.5 mg, 2.18 mmol) to the reaction liquid system, and heat the reaction liquid system to 80 ° C for 3.5 hours. After the reaction is completed, the reaction liquid is precipitated in an acetone solution to obtain 4.5 g of polyvinyl alcohol derivative P1′ containing a 1,4-dihydropyridine structure.

[0114] P1′ contains the following structural units:

[0115]

[0116] Wherein R is a benzaldehyde side chain group, x is 0.59, y is 0.29, and z is 0.12.

[0117] Depend on Figure 6 Shown 1 From the H-NMR spectrum, it can be seen that the characteristic peak of the benzene ring appears at the chemical shift of 6.92-7.16 ppm, and the characteristic peak of nitrogen and hydrogen on the dihydropyridine ring appears at about 8.97 ppm. It can be seen that the target polyvinyl alcohol derivative P1′ containing a 1,4-dihydropyridine structure is obtained in this example.

[0118] Example 6

[0119] The reaction equation is Figure 1 shown.

[0120] Polyvinyl alcohol 1799 (1.0 g, hydroxyl molar amount about 22.5 mmol) was dissolved in anhydrous N-methylpyrrolidone (10 mL) to form a clear transparent solution, diketene (283.7 mg, 3.38 mmol) was added, and stirred at 25°C for 1 hour. Then 3,4-dihydroxybenzaldehyde (700.4 mg, 5.07 mmol), 5,5-dimethyl-1,3-cyclohexanedione (710.6 mg, 5.07 mmol), ammonium acetate (586.2 mg, 7.61 mmol), and glycine (38.5 mg, 0.51 mmol) were added to the reaction liquid system, and the reaction liquid system was heated to 70°C for 2.5 hours. After the reaction was completed, the reaction liquid was precipitated in an acetone solution to obtain 1.8 g of polyvinyl alcohol derivative P4′ containing a 1,4-dihydropyridine structure.

[0121] P4′ contains the following structural units:

[0122]

[0123] Wherein R is a side chain group of 3,4-dihydroxybenzaldehyde, x is 0.06, y is 0.93, and z is 0.01.

[0124] Depend on Figure 7 Shown 1 From the H-NMR spectrum, it can be seen that the characteristic peak of the benzene ring appears at the chemical shift of 6.30-6.58 ppm, and the characteristic peak of nitrogen and hydrogen on the dihydropyridine ring appears at about 8.87 ppm. It can be seen that the target polyvinyl alcohol derivative P4′ containing a 1,4-dihydropyridine structure is obtained in this example.

[0125] Comparative Example 1

[0126] Polyvinyl alcohol 0588 was used as comparative example 1, which does not contain a dihydropyridine structure.

[0127] Test Example: The polyvinyl alcohol derivatives described in Examples 1 to 4 and Comparative Example 1 were subjected to an antioxidant test:

[0128] Comparison of the antioxidant properties of Examples 1 to 4 and Comparative Example 1:

[0129] Antioxidant test results Figure 8 As shown, P2 and P4 quench free radicals fastest, and can quench 93% of free radicals within 1 minute; followed by P3, which quenches about 92.6% of free radicals within half an hour; and P1 quenches free radicals the slowest, and can only quench 63% of free radicals within half an hour; polyvinyl alcohol that has not been modified with antioxidants cannot quench free radicals at all. This shows that the polyvinyl alcohol derivatives obtained by the modification method of the present invention have different degrees of antioxidant capacity, and are expected to be used in food packaging, biomedicine, health care and other fields.

[0130] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.

[0131] All publications, patent applications, patents and other references mentioned in this specification are incorporated herein by reference. Unless otherwise defined, all technical and scientific terms used in this specification have the meanings conventionally understood by those skilled in the art. In the event of a conflict, the definition in this specification shall prevail.

[0132] When this specification uses the prefix "well-known to those skilled in the art", "prior art" or similar terms to introduce materials, substances, methods, steps, devices or components, etc., the objects introduced by the prefix cover those commonly used in the art when this application is filed, but also include those that are not commonly used at present but will become recognized in the art as being suitable for similar purposes.

[0133] In the context of the present specification, any matters or items not mentioned are directly applicable to those known in the art without any changes except those explicitly stated.

Claims

1. An antioxidant polyvinyl alcohol derivative containing a 1,4-dihydropyridine structure, the antioxidant polyvinyl alcohol derivative comprising a structural unit containing 1,4-dihydropyridine, a vinyl alcohol structural unit and a vinyl acetate structural unit; The structural unit containing 1,4-dihydropyridine is of formula I: The vinyl alcohol structural unit is of formula II: The vinyl acetate structural unit is of formula III: In formula I, R is phenyl, substituted phenyl, heterocyclic aromatic group or C1-C8 alkyl group, the substituted phenyl group is preferably 3-methoxy-4-hydroxyphenyl, p-hydroxyphenyl or 3,4-dihydroxyphenyl, and the heterocyclic aromatic group is preferably 2-thienyl; The molar percentages of the structural unit containing 1,4-dihydropyridine, the vinyl alcohol structural unit and the vinyl acetate structural unit are x, y and z respectively, and x+y+z=1; wherein, x+y=alcoholysis degree, the alcoholysis degree is 88-99%; preferably, x is 4-99 mol%, y is 0-95 mol%, and the rest is z; further preferably, x is 4-91 mol%, y is 8-95 mol%, and the rest is z; further preferably, x is 4-60 mol%, y is 25-95 mol%, and the rest is z.

2. A method for preparing an antioxidant polyvinyl alcohol derivative containing a 1,4-dihydropyridine structure as claimed in claim 1, comprising the following steps: (1) dissolving polyvinyl alcohol in an anhydrous organic solvent, adding diketene to react to obtain a polyvinyl alcohol derivative containing β-diketone; (2) In the presence of a catalyst, an aldehyde compound, an ammonia source compound and a 1,3-diketone compound are added to the polyvinyl alcohol derivative containing β-diketone obtained in step (1) to carry out a Hantzsch reaction to obtain the antioxidant polyvinyl alcohol derivative containing a 1,4-dihydropyridine structure.

3. The method for preparing the antioxidant polyvinyl alcohol derivative containing 1,4-dihydropyridine structure according to claim 2, characterized in that: Step (1), The degree of polymerization of the polyvinyl alcohol is 500-1700, and the degree of alcoholysis is 88-99%; and / or, The anhydrous organic solvent is at least one of anhydrous N-methylpyrrolidone, anhydrous dimethyl sulfoxide, and anhydrous N,N-dimethylformamide.

4. The method for preparing the antioxidant polyvinyl alcohol derivative containing 1,4-dihydropyridine structure as claimed in claim 2, characterized in that: Step (1), The mass of the polyvinyl alcohol and the volume of the solvent are 0.05 to 0.3 g / ml, preferably 0.08 to 0.2 g / ml; and / or, The molar ratio of the hydroxyl group in the polyvinyl alcohol to the diketene is 1:(0.01-1), preferably 1:(0.1-0.9); and / or, The reaction temperature is 25 to 40°C, preferably 25 to 35°C; and / or, The reaction time is 1 to 3 hours, preferably 1 to 2 hours.

5. The method for preparing the antioxidant polyvinyl alcohol derivative containing 1,4-dihydropyridine structure as claimed in claim 2, characterized in that: Step (2), The catalyst is an amino acid catalyst or other weakly acidic catalyst, preferably glycine, proline or phenylboronic acid; and / or, The aldehyde compound is at least one of benzaldehyde, substituted benzaldehyde, heterocyclic aromatic aldehyde, and C1-C8 fatty aldehyde, the substituted benzaldehyde is preferably at least one of vanillin, p-hydroxybenzaldehyde, and 3,4-dihydroxybenzaldehyde, and the heterocyclic aromatic aldehyde is preferably 2-thiophenecarboxaldehyde; and / or, The ammonia source compound is at least one of ammonium acetate, ammonium carbonate and ammonia water; and / or, The 1,3-diketone compound is at least one of 1,3-cyclohexanedione and its derivatives, preferably at least one of 1,3-cyclohexanedione, 5-methyl-1,3-cyclohexanedione and 5,5-dimethyl-1,3-cyclohexanedione.

6. The method for preparing the antioxidant polyvinyl alcohol derivative containing 1,4-dihydropyridine structure as claimed in claim 2, characterized in that: Step (2), The molar ratio of the aldehyde compound, the ammonia source compound and the 1,3-diketone compound is 1:(1-2):(1-1.2), preferably 1:(1.2-1.6):(1-1.2), more preferably 1:(1.2-1.6):1; and / or, The molar ratio of the aldehyde compound to diketene is (1-2):1, preferably (1.1-1.5):1; and / or, The molar ratio of the catalyst to the aldehyde compound is (0.05-0.2):1, preferably (0.1-0.15):1; and / or, The reaction temperature is 70 to 90°C, preferably 70 to 80°C; and / or, The reaction time is 2 to 5 hours, preferably 2 to 4 hours.

7. The method for preparing the antioxidant polyvinyl alcohol derivative containing 1,4-dihydropyridine structure as claimed in claim 2, characterized in that: After the polyvinyl alcohol derivative containing β-diketone is obtained in step (1), it can be directly subjected to step (2) for Hantzsch reaction without purification; and / or, Step (2) After the Hantzsch reaction is completed, the polyvinyl alcohol derivative containing a 1,4-dihydropyridine structure is collected by an organic solvent precipitation method.

8. The method for preparing the antioxidant polyvinyl alcohol derivative containing 1,4-dihydropyridine structure as claimed in claim 7, characterized in that: The organic solvent is at least one of methanol, ethanol, acetone and acetonitrile.

9. An antioxidant polyvinyl alcohol derivative containing a 1,4-dihydropyridine structure obtained by the preparation method according to any one of claims 2 to 8.

10. Use of the antioxidant polyvinyl alcohol derivative containing 1,4-dihydropyridine structure as claimed in claim 1 or 9 in the fields of medicine, health and food packaging.

Citation Information

Patent Citations

  • Polyethylene alcoholic compound containing single functionalization group and preparation method thereof

    CN104558307A

  • Synthesis method of pyridine derivatives in polyethylene glycol

    CN105884681A

  • Anti-X-ray water-soluble polymer containing 1, 4-dihydropyridine structure and preparation method thereof

    CN111004359A

  • 1, 4-dihydropyridine polymer as well as high-throughput preparation method and application thereof

    CN111440260A

  • Modified vinyl alcohol-based polymer, modified vinyl ester-based polymer and methods for producing them