Double-gradient butylbenzene copolymer as well as preparation, application and product thereof

By developing S→B-(S/B)-B→S polymers with three-stage block structure and variable temperature polymerization characteristics, the processing complexity and performance of traditional styrene-butadiene copolymers in sole preparation are solved. The best problem is to realize the production of high-end shoe materials with convenient processing, excellent performance and low cost.

CN119019625AActive Publication Date: 2024-11-26CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310594820.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-11-26
Estimated Expiration
2043-05-25

AI Technical Summary

Technical Problem

Traditional styrene-butadiene copolymers have problems such as complex processing, poor performance, high cost and poor heat resistance when preparing soles. Especially, the soles are not easy to open, the details are not refined enough and at low temperatures due to injection molding. Easy to break.

Method used

Develop an S→B-(S/B)-B→S polymer, using three-stage block structure and variable temperature polymerization technology, to achieve injection molding vulcanization and improve dimensional stability by controlling the S/B content and proportion of each section. , wear resistance and other properties.

Benefits of technology

It realizes a styrene butadiene copolymer with easy processing and excellent performance, with excellent dimensional stability, tear resistance and transparency, which reduces costs and solves the problems of complexity and poor heat resistance in traditional processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004246747060000091
    Figure BDA0004246747060000091
  • Figure BDA0004246747060000101
    Figure BDA0004246747060000101
Patent Text Reader

Abstract

The invention belongs to the field of polymers, and particularly discloses an S-B-(S / B)-B-S polymer which is a triblock polymer, the first block is an S-B gradual change block, the second block is an S / B random block, and the third block is a B-S gradual change block. In the S-B-(S / B)-B-S polymer, the total molecular weight is 70000-120000, the content of styrene is 30-60wt%, and the content of vinyl is 15-40wt%; wherein in the first section, the content of S is 5-10 wt%, and the content of B is 2-5 wt%; in the second section, the content of S is 22-43 wt%, and the content of B is 40-60 wt%. The invention also comprises preparation and application of the copolymer. The polymer disclosed by the invention has brand new structural characteristics and excellent comprehensive performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and specifically relates to the technical field of butadiene-styrene copolymers. Technical Background

[0002] Traditional styrene-butadiene copolymers generally include two types of products, SBS and SSBR. The processes for preparing the soles of these two types of products are completely different. SBS generally adopts the injection mold vulcanization molding process to prepare the soles, while SSBR generally adopts the high-pressure mold vulcanization molding process to prepare the soles. The two preparation processes have their own characteristics: the injection mold vulcanization molding process of rubber has the characteristics of high feeding accuracy, short operation time, and fast vulcanization speed, which can greatly reduce labor costs and improve the economic benefits of enterprises. The rubber injected by the injection machine has a higher density, and the hardness, tensile strength and elongation at break are improved, and the permanent deformation at break is small, which has a positive effect on improving the performance of rubber products; while the injection mold vulcanization molding process has a short production cycle, high efficiency, strong adaptability, and easy automation.

[0003] Vulcanized rubber soles are soft, extremely elastic, not prone to aging and cracking, and heat-resistant, and can be used in various sports, but their production process is relatively complex. Injection-molded rubber soles are not easy to debond, and due to the simple production process, the details are generally not refined enough, and the special composition of the soles makes them prone to breaking and hardening at low temperatures. At the same time, during production, the soles are prone to forming uneven blocks, so the wearing comfort is relatively poor.

[0004] The inventor has been committed to the research and development of styrene-butadiene copolymers for many years, hoping to develop a styrene-butadiene copolymer material that is easy to process and has excellent performance, so as to combine the performance and processing advantages of SBS injection vulcanization molded soles and SSBR injection mold vulcanization molded soles to meet the market's higher requirements for shoe materials. Summary of the invention

[0005] In view of the shortcomings of the prior art, the first purpose of the present invention is to provide a S→B-(S / B)-B→S polymer (also referred to as a double gradient butadiene-styrene copolymer in the present invention), aiming to provide a new polymer that can be injection molded and vulcanized and has excellent dimensional stability, wear resistance and other properties.

[0006] The second object of the present invention is to provide a method for preparing the S→B-(S / B)-B→S polymer.

[0007] The third object of the present invention is to provide the use of the S→B-(S / B)-B→S polymer in the preparation of vulcanized products such as shoe soles.

[0008] The fourth object of the present invention is to provide a polymer composition comprising the S→B-(S / B)-B→S polymer and a rubber product thereof.

[0009] A S→B-(S / B)-B→S polymer is a triblock polymer, wherein the first segment is an S→B gradient block, the second segment is an S / B random block, and the third segment is a B→S gradient block;

[0010] The S→B-(S / B)-B→S polymer has a total molecular weight of 70,000-120,000, a styrene content of 30-60wt.%, and a vinyl content of 15-40wt%. The S content in the first section is 5-10wt%, and the B content is 2-5wt%. The S content in the second section is 22-43wt%, and the B content is 40-60wt%.

[0011] The present invention provides a new polymer with a special double gradient structure of (S→B) and (B→S), and further cooperates with the control of the S / B content and ratio of each section to achieve synergy and unexpectedly achieve injection molding vulcanization. Not only that, it is also beneficial to improve the dimensional stability, wear resistance and other properties of the prepared products.

[0012] In the present invention, the S→B block described in the first paragraph refers to a copolymer block formed by styrene and butadiene, and in this block, the starting segment is polystyrene, and as the chain segment is extended, the polystyrene content gradually decreases, and the polybutadiene content gradually increases. The S / B random block described in the second paragraph refers to a block formed by random copolymerization of styrene and butadiene. The B→S block described in the third paragraph refers to a copolymer block formed by styrene and butadiene, and in this block, as the chain segment is extended, the polybutadiene content gradually decreases, the polystyrene content gradually increases, and the terminal is a polystyrene structure.

[0013] In the present invention, the special double gradient structure and the joint control of the S / B content of each segment are the key to synergistically improving its performance.

[0014] In the present invention, the content of S or B in each segment is based on the total monomer content (S+B).

[0015] Preferably, the content of S in the first section is 5-10wt.%, the content of S in the second section is 28-36wt.%, the balance is S in the third section, and the total S content of the first to third sections is 40-50wt.%. In addition, the content of B in the first section is 2-5wt.%, the content of B in the second section is 40-55wt.%, and the balance is B in the third section.

[0016] Preferably, the molecular weight of the S→B gradient block (first segment) is 5000-12000, wherein the molecular weight of the initial polystyrene is 500-1000. The molecular weight of the second segment is 50000-80000. The molecular weight of the B→S gradient block (third segment) is 3000-6000, wherein the molecular weight of the terminal polystyrene is 200-1000.

[0017] The present invention also provides a method for preparing the S→B-(S / B)-B→S polymer, comprising the steps of: subjecting a solution containing an initiator, a regulator, styrene and butadiene required in the first stage to first stage polymerization at a temperature below 10°C (preferably -10°C to 10°C); then continuously adding a mixed monomer containing butadiene and styrene required in the second stage to perform second stage polymerization, wherein the temperature of the second stage polymerization is 80°C to 130°C (preferably 100°C to 110°C); then adding styrene and butadiene monomers required in the third stage to perform third stage polymerization, thereby obtaining the S→B-(S / B)-B→S polymer, wherein the temperature of the third stage polymerization is 65°C to 90°C.

[0018] In order to successfully prepare the double gradient polymer and solve the problem of preparing the double gradient polymer, the present invention has been found to innovatively provide a three-stage variable temperature polymerization idea, which polymerizes the required amount of styrene and butadiene at the required low temperature in the first stage, and then raises the temperature to carry out the second stage polymerization and the third stage polymerization. On this basis, the S / B addition method, ratio and temperature of each stage polymerization are further coordinated. This can solve the preparation problem of the polymer and facilitate the successful preparation of the double gradient polymer. Not only that, it also helps to improve the performance of the obtained polymer.

[0019] In the present invention, the combination of the variable temperature polymerization method and the S / B addition method and ratio in the preparation process is the key to the coordinated preparation of the new polymer and the improvement of its performance.

[0020] In the present invention, the S and B required for the first stage are mixed at once and then polymerized at low temperature in the presence of an initiator and a regulator, which is conducive to the successful preparation of the double gradient polymer and improves its performance.

[0021] In the present invention, the initiator may be a conventional anionic initiator in the industry, for example, alkyl lithium, and further butyl lithium.

[0022] In the present invention, the amount of the initiator can be adjusted according to the polymerization requirements, for example, it can be 1.0-1.7 mmol / 100 g dry glue.

[0023] In the present invention, the solvent in the first polymerization stage can be any conventional solvent in the industry, for example, it can be at least one of n-hexane, cyclohexane, hexane, pentane, and the like.

[0024] In the present invention, the regulator can be at least one of THF, ether, anisole, crown ether, cryptand, dioxane, tetramethylethylenediamine, triethylamine, etc., which are well known in the industry. In addition, the amount of the regulator can be adjusted according to the requirements of the prepared 1,2 structure, for example, it can be 50-200 ppm (content in the solvent).

[0025] In the present invention, the time of the first stage polymerization is 60 min to 90 min.

[0026] In the present invention, in the first polymerization stage, styrene is used in an amount of 5 to 10 wt% of the total monomers, and butadiene is used in an amount of 2 to 5 wt% of the total monomers.

[0027] In the present invention, after the first stage of polymerization is completed, styrene and butadiene mixed monomers are directly and continuously added to the polymerization system, and the temperature is raised to carry out the second stage of polymerization. In the present invention, the polymerization is gradually increased from the low temperature of the first stage to the relatively high temperature of the second stage, and the S / B addition method and the combined control of the dosage are combined, which is conducive to forming the special structure and a new polymer with excellent performance.

[0028] In the present invention, in the second polymerization stage, styrene is used in an amount of 22-43 wt% of the total monomers, and butadiene is used in an amount of 40-60 wt% of the total monomers.

[0029] In the present invention, the second stage polymerization time is 30 min to 60 min.

[0030] In the present invention, after the second stage polymerization is completed, the remaining styrene and butadiene required are added to carry out the third stage polymerization.

[0031] In the third polymerization stage of the present invention, the required styrene and butadiene monomers can be added at one time.

[0032] Preferably, the third stage polymerization time is 30 min to 60 min.

[0033] In the present invention, the polymerization reaction can be quenched based on existing means to obtain the new polymer.

[0034] The present invention also provides the application of the S→B-(S / B)-B→S polymer to prepare rubber products, preferably vulcanized rubber products, further preferably injection molded vulcanized rubber products, and further injection molded vulcanized sole rubber products.

[0035] In the present invention, the S→B-(S / B)-B→S polymer can be made into any desired product based on known principles and means.

[0036] The present invention also provides a polymer composition comprising the S→B-(S / B)-B→S polymer.

[0037] In the present invention, the polymer composition is further allowed to contain at least one of a bridging agent, a cross-linking aid, a cross-linking aid, an antioxidant, a regenerated rubber, and a filler.

[0038] For example, an exemplified polymer composition of the present invention is a composition comprising a S→B-(S / B)-B→S polymer, a bridging agent, a crosslinking aid A, a crosslinking aid B, an antioxidant, reclaimed rubber and a filler.

[0039] The bridging agent, crosslinking agent A, crosslinking agent B, antioxidant, reclaimed rubber and filler can all be ingredients known in the industry. For example, the bridging agent is at least one of BPO, DTBP, DCP and BIBP. The crosslinking agent A is at least one of ZnO, MgO and stearic acid. The crosslinking agent B is at least one of TMPTMA, TMPTA, EGDA, EGDMA, ZDMA and TAIC. The antioxidant is at least one of antioxidant 1076, antioxidant 1010, antioxidant 168 and antioxidant 626. The filler is at least one of white carbon black, carbon black, silicate and carbonate.

[0040] The polymer composition embodiment further enumerated by the present invention has the weight ratio of each component as follows:

[0041] S→B-(S / B)-B→S polymer, 50 parts

[0042] 0.5-1.0 part of bridging agent;

[0043] Crosslinking agent A 0.5-2.0 parts

[0044] Crosslinking agent B 0.5-2.0 parts

[0045] Antioxidant 0.1~0.5 parts

[0046] 10-20 parts of recycled rubber

[0047] 5-10 parts of filler.

[0048] The present invention also provides a vulcanized rubber product, which is obtained by vulcanizing the polymer composition containing the novel polymer described in the present invention.

[0049] In the present invention, the polymer composition of the present invention can be vulcanized based on known means to obtain the desired product.

[0050] For example, in one embodiment of the present invention, the vulcanized rubber product is vulcanized by an injection mold vulcanization molding process, and further, the vulcanized rubber product is a sole vulcanized by an injection mold vulcanization molding process.

[0051] Beneficial Effects

[0052] 1. The present invention provides a polymer with a completely new structure, which is based on a special double gradient structure and the joint control of the S / B content and ratio of each segment, and can achieve synergy and improve the performance of the polymer. For example, the polymer has good processing fluidity and can meet the requirements of injection molding processing and performance. The obtained product has good dimensional stability and good gloss.

[0053] 2. The present invention is based on the variable temperature three-stage polymerization concept, and further cooperates with the joint control of the monomer addition method, proportion and polymerization temperature, which can achieve synergy and successfully solve the problems faced by the polymer preparation of the present invention. The polymer can be successfully prepared. Not only that, it is also beneficial to improve the performance of the prepared polymer.

[0054] 3. Products prepared by the polymer with the new structure described in the present invention have excellent properties. For example, the prepared soles have good tear strength, wear resistance, dimensional stability and transparency, are easy to process, and have low cost. High-end shoe materials that combine functionality and fashion can be prepared.

[0055] In addition, the polymer of the present invention can be prepared by injection molding, which solves the shortcomings of traditional SSBR vulcanization, which requires the addition of sulfur (with a strong odor and not environmentally friendly) and requires a high-pressure mold vulcanization molding process, complex processing and poor tear strength. DETAILED DESCRIPTION

[0056] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0057] The novel structure of the styrene-butadiene copolymer (labeled as: S→B-(S / B)-B→S polymer) of the present invention comprises three sections: the first section is a styrene-butadiene gradient structure (S→B section) which first initiates polystyrene, the second section is a styrene-butadiene random copolymer (S / B section), and the third section is a structure with butadiene-styrene gradient ends terminated with polystyrene (B→S section).

[0058] In the S→B-(S / B)-B→S polymer, the total combined styrene content is 30-60%, the total molecular weight is 70,000-120,000, and the vinyl content is 15-40%.

[0059] In one section of the structure: the total styrene content in one section is 5-10wt.%, the amount of combined butadiene is 2-5wt.%, the molecular weight of the first initiated polystyrene is 500-1000, and the gradual molecular weight of styrene-butadiene is 5000-12000.

[0060] In the second-stage structure, the total styrene content in the second stage is 22-43wt.%, the amount of butadiene combined is 40-60wt.%, it is a completely random structure, and the molecular weight is 50000-80000.

[0061] In the three-stage structure: the remaining styrene and butadiene are combined in the three stages (for example, the total styrene content in the three stages is 3-7%, and the amount of combined butadiene is 5-10%), the butadiene-styrene gradient molecular weight is 3000-6000, and the molecular weight of the terminal-capped polystyrene is 200-1000.

[0062] The synthetic method of the polymerization of the novel structure of the styrene-butadiene copolymer of the present invention is, for example:

[0063] 1) using alkyl lithium as an initiator and tetrahydrofuran as a regulator, polymerizing a styrene butadiene mixed monomer in a stage, wherein the initiation temperature is below 10° C., preferably -10° C. to 10° C., and the reaction time is 60 min to 90 min;

[0064] 2) Then, a mixed monomer of butadiene and styrene is added to carry out two-stage polymerization, the reaction temperature is 80°C to 130°C, and the reaction time is 30min to 60min;

[0065] 3) Add styrene to carry out three-stage styrene-butadiene mixed monomer polymerization at a reaction temperature of 65° C. to 90° C. for 30 min to 60 min;

[0066] Comparative Example 1

[0067] In a 5-liter stainless steel reactor with stirring, 3000 ml of cyclohexane and 0.3 ml of tetrahydrofuran were added, and 70 g of styrene was added. The temperature was adjusted to 65°C, and 11 ml (concentration of 0.4 mol / l) of initiator butyl lithium was added. The reaction was continued for 30 minutes. After the reaction was completed, 210 g of butadiene monomer was added, and then 70 g of styrene monomer was added. The reaction time was 30 minutes, and then the material was discharged. Then an antioxidant was added, and the water vapor was condensed and dried for use.

[0068] Example 1

[0069] In a 5-liter stainless steel reactor with stirring, 3000 ml of cyclohexane and 0.35 ml of tetramethylethylenediamine were added, 30 g of styrene and 15 g of butadiene were added, the temperature was adjusted to -5°C, and 11 ml (concentration of 0.4 mol / l) of initiator butyl lithium was added, and the reaction was carried out for 60 minutes. After the reaction, the reactor was heated to 100°C, and then 90 g of styrene and 185 g of butadiene were added continuously. After the reaction, the reactor temperature was 80°C, and 20 g of styrene and 10 g of butadiene were added again. The reaction time was 10-30 min, and the material was discharged. Then an antioxidant was added, and the water vapor was condensed and dried for use.

[0070] Example 2

[0071] In a 5-liter stainless steel reactor with stirring, 3000 ml of cyclohexane and 0.25 ml of dioxane, 30 g of styrene and 15 g of butadiene were added, the temperature was adjusted to -5°C, and 11 ml (concentration of 0.4 mol / l) of initiator butyl lithium was added, and the reaction was carried out for 60 minutes. After the reaction, the reactor was heated to 100°C, and then 125 g of styrene and 150 g of butadiene were added continuously. After the reaction, the reactor temperature was 80°C, and 20 g of styrene and 10 g of butadiene were added again. The reaction time was 10-30 min, and the material was discharged. Then an antioxidant was added, and the water vapor was condensed and dried for use.

[0072] Example 3

[0073] In a 5-liter stainless steel reactor with stirring, 3000 ml of cyclohexane and 0.3 ml of tetrahydrofuran were added, 30 g of styrene and 15 g of butadiene were added, the temperature was adjusted to -5°C, and 9 ml (concentration was 0.4 mol / l) of initiator butyl lithium was added, and the reaction was carried out for 60 minutes. After the reaction, the reactor was heated to 100°C, and then 90 g of styrene and 185 g of butadiene were added continuously. After the reaction, the reactor temperature was 80°C, and 20 g of styrene and 10 g of butadiene were added again. The reaction time was 10-30 min, and the material was discharged. Then an antioxidant was added, and the water vapor was condensed and dried for use.

[0074] Example 4

[0075] In a 5-liter stainless steel reactor with stirring, 3000 ml of cyclohexane and 0.5 ml of tetrahydrofuran were added, 25 g of styrene and 10 g of butadiene were added, the temperature was adjusted to -5°C, and 10 ml (concentration was 0.4 mol / l) of initiator butyl lithium was added, and the reaction was carried out for 60 minutes. After the reaction, the reactor was heated to 100°C, and then a mixed monomer of 100 g of styrene and 192 g of butadiene was continuously added. After the reaction, the reactor temperature was 80°C, and 15 g of styrene and 8 g of butadiene mixed monomer were added again. The reaction time was 10-30 min, and the material was discharged. Then an antioxidant was added, and the water vapor was condensed and dried for standby use.

[0076] Example 5

[0077] In a 5-liter stainless steel reactor with stirring, 3000 ml of cyclohexane and 0.3 ml of tetrahydrofuran were added, 25 g of styrene and 10 g of butadiene were added, the temperature was adjusted to -10°C, and 10 ml (concentration was 0.4 mol / l) of initiator butyl lithium was added, and the reaction was carried out for 60 minutes. After the reaction, the reactor was heated to 110°C, and then a mixed monomer of 100 g of styrene and 192 g of butadiene was continuously added. After the reaction, the reactor temperature was 70°C, and 15 g of styrene and 8 g of butadiene mixed monomer were added again. The reaction time was 10-30 min, and the material was discharged. Then an antioxidant was added, and the water vapor was condensed and dried for use.

[0078] Comparative Example 2 (double gradient structure not formed in the first section)

[0079] In a 5-liter stainless steel reactor with stirring, 3000 ml of cyclohexane and 0.3 ml of tetrahydrofuran were added, and 45 g of styrene was added. The temperature was adjusted to 65°C, and then 11 ml (concentration of 0.4 mol / l) of initiator butyl lithium was added. The reaction was continued for 60 minutes, and then 110 g of styrene and 165 g of butadiene mixed monomers were added continuously. After the reaction, the reactor temperature was 80°C, and 20 g of styrene and 10 g of butadiene mixed monomers were added again. The reaction time was 10-30 min, and the material was discharged. Then, an antioxidant was added, and the water vapor was condensed and dried for use.

[0080] Comparative Example 3 (the third section does not form a double gradient structure)

[0081] In a 5-liter stainless steel reactor with stirring, 3000 ml of cyclohexane and 0.3 ml of tetrahydrofuran, 30 g of styrene and 15 g of butadiene were added, the temperature was adjusted to -5°C, and 11 ml (concentration of 0.4 mol / l) of initiator butyl lithium was added, and the reaction was carried out for 60 minutes. After the reaction was completed, the reactor was heated to 100°C, and then a mixed monomer of 115 g of styrene and 170 g of butadiene was continuously added. After the reaction was completed, 30 g of styrene monomer was added at a time. The reaction time was 10-30 min, and the material was discharged. Then an antioxidant was added, and the water vapor was condensed and dried for use.

[0082] Comparative Example 4 (S / B=20 / 80)

[0083] In a 5-liter stainless steel reactor with stirring, 3000 ml of cyclohexane and 0.3 ml of tetrahydrofuran were added, 12 g of styrene and 24 g of butadiene were added, the temperature was adjusted to -5°C, and 11 ml (concentration of 0.4 mol / l) of initiator butyl lithium was added, and the reaction was carried out for 60 minutes. After the reaction, the reactor was heated to 100°C, and then 50 g of styrene and 252 g of butadiene were added continuously. After the reaction, the reactor temperature was 80°C, and 8 g of styrene and 4 g of butadiene were added again. The reaction time was 10-30 min, and the material was discharged. Then an antioxidant was added, and the water vapor was condensed and dried for use. It has no physical properties at room temperature.

[0084] Comparative Example 5 (the first stage polymerization was not carried out at low temperature)

[0085] In a 5-liter stainless steel reactor with stirring, add 3000 ml cyclohexane and 0.3 ml tetrahydrofuran, add 30 g styrene and 15 g butadiene, adjust the temperature to 65°C, then add 11 ml (concentration is 0.4 mol / l) of initiator butyl lithium, react for 60 minutes, then add 125 g styrene and 150 g butadiene mixed monomer at about 60°C after the reaction is completed, then add 20 g styrene and 10 g butadiene mixed monomer at about 75°C at a time, react for 10-30 minutes, then add antioxidant, condense water vapor, dry and set aside. (The middle section is uneven, the tear resistance is poor, the sample is sticky, etc.).

[0086] Table 1 Performance test results of polymers obtained in various embodiments and comparative examples

[0087]

[0088] The following vulcanization studies were conducted on the polymers prepared in each case, wherein the polymer formulations were:

[0089] 50 parts of styrene-butadiene copolymer prepared in each case

[0090] Bridging agent or cross-linking agent BP0 / DTBP, 1 part

[0091] Crosslinking agent ZnO, 1 part

[0092] Crosslinking aid TMPTMA, 1 part

[0093] Antioxidant 1076 / 1010, 0.2 parts

[0094] Antioxidant 168 or 626, 0.2 parts

[0095] Recycled rubber, 15 parts

[0096] White carbon black, 8 parts

[0097] In the present invention, the polymer composition of the present invention can be vulcanized based on existing means to obtain the desired products. For example, a typical injection mold vulcanization molding process of a styrene-butadiene copolymer composition includes the following steps: a 600t injection vulcanizer is selected, the bottom plate and the top plate are loaded into the mold, and the mold is closed, and the mixed rubber is injected into the mold cavity through the injection vulcanizer. During the production process, the screw temperature is 60°C-110°C, the vulcanization (mold) temperature is (170±5)°C for the upper plate and (170±5)°C for the lower plate, the vulcanization time will be determined according to the simulation analysis results, and the vulcanization pressure is 15MPa.

[0098] The test results are shown in Table 2:

[0099] Table 2 Performance of the polymerization vulcanization of the embodiment

[0100]

[0101] It can be seen that the vulcanized polymer prepared by the method of the present invention has excellent comprehensive properties.

Claims

1. A S→B-(S / B)-B→S polymer, characterized in that: It is a triblock polymer, wherein the first segment is an S→B gradient block, the second segment is an S / B random block, and the third segment is a B→S gradient block; The S→B-(S / B)-B→S polymer has a total molecular weight of 70,000-120,000, a styrene content of 30-60wt.%, and a vinyl content of 15-40wt%. The S content in the first section is 5-10wt%, and the B content is 2-5wt%. The S content in the second section is 22-43wt%, and the B content is 40-60wt%.

2. The S→B-(S / B)-B→S polymer according to claim 1, characterized in that The molecular weight of the S→B gradient block is 5000-12000.

3. The S→B-(S / B)-B→S polymer according to claim 1, characterized in that The molecular weight of the second segment is 50,000-80,000.

4. The S→B-(S / B)-B→S polymer according to claim 1, characterized in that The molecular weight of the B→S gradient block is 3000-6000.

5. The S→B-(S / B)-B→S polymer according to any one of claims 1 to 4, characterized in that The molecular weight of the polystyrene at the beginning of the first section is 500-1000; the molecular weight of the polystyrene at the end of the third section is 200-1000.

6. A method for preparing the S→B-(S / B)-B→S polymer according to any one of claims 1 to 5, characterized in that: A solution containing an initiator, a regulator, styrene and butadiene required in the first stage is subjected to first stage polymerization at a temperature below 10°C; then a mixed monomer containing butadiene and styrene required in the second stage is continuously added to carry out second stage polymerization, wherein the temperature of the second stage polymerization is 80°C to 130°C; then styrene and butadiene monomers required in the third stage are added to carry out third stage polymerization to obtain the S→B-(S / B)-B→S polymer, wherein the temperature of the third stage polymerization is 65°C to 90°C.

7. The preparation method according to claim 6, characterized in that: The initiator is an alkyl lithium, preferably butyl lithium; Preferably, the amount of the initiator used is 1.0-1.7 mmol / 100 g of dry glue.

8. The preparation method according to claim 6, characterized in that: The regulator is at least one of THF, ether, anisole, crown ether, cryptand, dioxane, tetramethylethylenediamine, triethylamine, etc.; Preferably, the amount of the regulator is 50-200 ppm.

9. The preparation method according to claim 6, characterized in that: In the first polymerization stage, styrene and butadiene are added at once; Preferably, in the third polymerization stage, styrene and butadiene are added at once; Preferably, the first stage polymerization time is 60 min to 90 min; Preferably, the second stage polymerization time is 30 min to 60 min; Preferably, the third stage polymerization time is 30 min to 60 min.

10. Use of the S→B-(S / B)-B→S polymer according to any one of claims 1 to 5, characterized in that: The rubber product is prepared into rubber products, preferably vulcanized rubber products, preferably injection molded vulcanized rubber products, and further injection molded vulcanized sole rubber products.

11. A polymer composition comprising the S→B-(S / B)-B→S polymer according to any one of claims 1 to 5.

12. The polymer composition according to claim 11, characterized in that It also contains at least one of a bridging agent, a cross-linking aid, a cross-linking aid, an antioxidant, regenerated rubber, and a filler.

13. The polymer composition according to claim 12, characterized in that A composition comprising a S→B-(S / B)-B→S polymer, a bridging agent, a crosslinking aid A, a crosslinking aid B, an antioxidant, reclaimed rubber and a filler; Preferably, the bridging agent is at least one of BPO, DTBP, DCP and BIBP; Preferably, the crosslinking aid A is at least one of ZnO, MgO and stearic acid; Preferably, the crosslinking aid B is at least one of TMPTMA, TMPTA, EGDA, EGDMA, ZDMA, and TAIC; Preferably, the antioxidant is at least one of antioxidant 1076, antioxidant 1010, antioxidant 168 or antioxidant 626; Preferably, the filler is at least one of white carbon black, carbon black, silicate and carbonate.

14. The polymer composition according to claim 12 or 13, characterized in that The weight ratio of each component is: S→B-(S / B)-B→S polymer, 50 parts 0.5-1.0 part of bridging agent; Crosslinking agent A0.5-2.0 parts Crosslinking agent B 0.5-2.0 parts Antioxidant 0.1~0.5 parts 10-20 parts of recycled rubber 5-10 parts of filler.

15. A vulcanized rubber product, characterized in that: Obtained by vulcanizing the polymer composition according to any one of claims 11 to 14; Preferably, the vulcanized rubber product is vulcanized by injection molding vulcanization process; Preferably, the vulcanized rubber product is a shoe sole vulcanized by injection mold vulcanization molding process.

Citation Information

Patent Citations

  • Two-stage material-feeding random gradually-varied butylbenzene co-polymer and preparation method thereof

    CN104292408A

  • Styrene-butadiene copolymer and preparation method thereof, and application of styrene-butadiene copolymer in shoe soles

    CN107236101A

  • Diblock butylbenzene copolymer, preparation method thereof and application of diblock butylbenzene copolymer in transparent vulcanized sole

    CN116023605A

  • Vulcanizable shoe soling composition

    US4238383A