Allyl polyphenyl ether resin and preparation method thereof as well as flexible low-dielectric material and preparation method thereof

By introducing diallyl structure and click reaction in polyphenylene ether, a high content of allyl polyphenylene ether resin was prepared, which solved the problems of high dielectric constant and low flexibility of polyphenylene ether resin in the field of flexible low dielectric materials. , realizes the combination of low dielectric performance and high flexibility, and improves the processability and application value of materials.

CN119019675AActive Publication Date: 2024-11-26BEIJING UNIV OF CHEM TECH +1

Patent Information

Application Number
CN202411251487.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-07
Publication Date
2024-11-26
Estimated Expiration
2044-09-07

AI Technical Summary

Technical Problem

The existing polyphenylene ether resins are limited in the field of flexible low-dielectric materials. Due to their high dielectric constant, low flexibility and processing difficulties, and the commonly used modification methods are difficult to effectively improve the allyl content and reactivity.

Method used

By introducing a diallyl structure in polyphenylene ether molecules by amination reaction and performing click reaction with dithiol, a high-content allyl polyphenylene ether resin is prepared, and the processability is improved by combining solvent method and reducing the dielectric constant. and dielectric loss.

Benefits of technology

It realizes the low dielectric properties and high flexibility of the resin, maintains the hydrophobic properties of polyphenylene ether, and improves the processability and practical application value of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019675A_ABST
    Figure CN119019675A_ABST
Patent Text Reader

Abstract

The invention discloses allyl polyphenyl ether resin and a preparation method thereof, and a flexible low-dielectric material and a preparation method thereof. The preparation method of the flexible low-dielectric material comprises the following steps: reacting polyphenyl ether resin with a brominating agent to obtain brominated polyphenyl ether resin, and performing amination reaction on the brominated polyphenyl ether resin and allyl amine to obtain polyphenyl ether resin with high allyl content; the preparation method comprises the following steps: under the action of a photoinitiator, carrying out thiol-ene click chemical reaction on allyl polyphenyl ether resin and dithiol under an ultraviolet light condition, and then heating and curing to obtain the flexible low-dielectric material. The preparation method is simple and convenient, the raw materials are easy to obtain, the preparation period is short, and the low dielectric property of the cured flexible material is stable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer material synthesis and preparation, and in particular to an allyl polyphenylene ether resin and a preparation method thereof, a flexible low dielectric material and a preparation method thereof. Background Art

[0002] Polyphenylene ether resin is an engineering plastic with excellent dimensional stability, heat resistance, insulation and low dielectric properties. It is often used in electronic packaging, insulation materials, equipment parts and other fields. However, with the development of flexible electronic packaging technologies such as smart wearables, biomedicine, flexible displays, and new energy sources, the demand for corresponding packaging materials is becoming more and more urgent, and the performance requirements for flexible packaging materials are becoming higher and higher. At present, general-purpose polyphenylene ether has no active functional groups and is generally mixed with other resins. However, it has high melt viscosity, poor fluidity, difficulty in processing and molding, and poor compatibility with other resins, which limits its industrial application. In addition, the polyphenylene ether molecular chain contains a large number of benzene rings. This rigid structure also limits its application in the field of flexible low dielectric materials. Therefore, it is of great significance to develop polyphenylene ether resins with active functional groups as flexible packaging materials.

[0003] At present, commonly used flexible electronic materials include polyvinyl alcohol (PVA), polyester (PET), polyimide (PI), and polyethylene glycol naphthalate, but these materials contain polar groups such as alcohol hydroxyl, ester and amine groups, have a high polarizability, and have a high dielectric constant, which is not suitable for low dielectric scene applications. As for the modification of polyphenylene ether materials, polystyrene (PS), high impact polystyrene (HIPS), ternary copolymer ethylene propylene rubber (EPDM), etc. are mainly used for blending to improve fluidity and reduce dielectric constant. Chinese patent application CN115725167A (Cao Yanxiao, Li Xianhong, Ran Guowen, Lan Xiucai, Zhou Shufen) A polyphenylene ether-based composite material with low dielectric constant and low dielectric loss and its preparation method, Chinese patent 2023.03.03, a polyphenylene ether-based composite material with low dielectric constant and low dielectric loss is prepared by polyphenylene ether resin, polystyrene resin, fluororesin, hollow glass microspheres, etc., while satisfying the material with low dielectric properties, and can maintain its mechanical strength and toughness. However, this method obtains low-dielectric alloy materials by blending a variety of resins and additives, which has poor flexibility, and the raw materials used have no active functional groups, making it difficult to form effective adhesion to the substrate. In addition, active functional groups are introduced into polyphenylene ether resins through modifications such as end group esterification, epoxidation, and vinylization to improve the reaction activity. China's patent application CN117487155A (Xiao Zhichun) is a method for preparing a modified low-molecular-weight bifunctional polyphenylene ether oligomer with vinyl-terminated polyphenylene ether, Chinese patent 2024.02.02, vinyl-terminated low-molecular-weight polyphenylene ether by saponification reaction, introducing unsaturated double bonds, and using it together with styrene, allyl methacrylate and other unsaturated polyester monomers and resins, curing and cross-linking in a hot oxygen environment, and preparing a material with strong dielectric properties, good insulation properties, and extremely low hygroscopicity, which is suitable for PCB boards, copper-clad boards, 5G, and 6G electronic power packaging. However, this method is to vinyl-terminate polyphenylene ether, which has a low double bond content and fewer active sites, affecting the cured network. Allyl methacrylic acid and unsaturated polyester monomer used in composite all contain polar functional groups, increase molecular polarizability, and are unfavorable for reducing dielectric properties. In addition, allyl polyphenyl ether is as thermosetting resin, and its allyl content directly affects material cross-linking density, heat resistance and mechanical property, and existing allylated polyphenyl ether industrial product (Asahi Chemical S2100) is to carry out lithiation reaction by polyphenyl ether and n-butyl lithium, and then generate allylated polyphenyl ether with propylene bromide reaction. This thermosetting allylated polyphenyl ether tool dielectric constant is low, and circuit signal transmission speed is higher than epoxy resin, polyimide resin, cyanate resin characteristics. But this method is to improve allyl replacement rate, and its reaction time, reaction condition control is stricter, and in corresponding lithiated body active site, can only introduce an allyl group, is unfavorable for promoting allyl content, thereby limits the thermosetting performance of further promoting material. Summary of the invention

[0004] In view of the problems in the background technology, the object of the present invention is to provide an allyl polyphenylene ether resin and a preparation method thereof, a flexible low dielectric material and a preparation method thereof, by preparing a novel side allyl polyphenylene ether resin, a diallyl structure is introduced in the polyphenylene ether molecular structure by amination reaction, the content of the active functional group allyl in the resin is greatly improved, and by clicking with dithiol in a solvent, the intrinsic high flexibility and low dielectric properties after curing. The resin does not contain a strong polar group and has a flexible structure of a polyphenylene ether rigid skeleton and dithiol at the same time, therefore, the structure can reduce the dielectric constant and dielectric loss of the resin, and maintain excellent flexibility and hydrophobicity, and the solvent method improves its processability and the interaction between various fillers, which is of great significance to the practical application of the flexible electronics industry.

[0005] One of the objects of the present invention is to provide a method for preparing an allyl polyphenylene ether resin, which comprises the following steps: (1) reacting polyphenylene ether with a brominating agent to obtain brominated polyphenylene ether; and (2) reacting brominated polyphenylene ether with an allyl compound to obtain an allyl polyphenylene ether resin.

[0006] Optionally, in step (1), polyphenylene ether and tetrahydrofuran are dissolved in a mass ratio of 1:(3-5) by a solvent method. After sufficient dissolution, polyphenylene ether, brominating agent and dibenzoyl peroxide are added in a molar ratio of 1:(20-30):(0.2-0.5) for reaction. The reaction temperature is maintained at 70-80°C. The reaction is carried out under the protection of high-purity nitrogen for 2 hours. After cooling to room temperature, anhydrous methanol is added for washing. The precipitate is separated to obtain a precipitate, which is vacuum dried. The washing and drying are repeated 3-4 times. Finally, the solid brominated polyphenylene ether resin is obtained by vacuum drying.

[0007] Optionally, the brominated polyphenylene ether prepared according to step (1) is dissolved in tetrahydrofuran in a mass ratio of 1:(3-5). After sufficient dissolution, the brominated polyphenylene ether, the allyl compound and potassium carbonate are added in a molar ratio of 1:(10-20):(3-5) for reaction. The reaction temperature is maintained at 45-50° C. The reaction is carried out under the protection of high-purity nitrogen for 8 hours. After cooling to room temperature, anhydrous methanol is added for washing, and the precipitate is separated to obtain a precipitate, which is vacuum dried. The washing and drying are repeated 3-4 times, and finally vacuum dried to obtain a solid allyl polyphenylene ether resin (ALPPO).

[0008] Optionally, in step (1), the brominating agent is at least one of N-bromosuccinimide, N-bromo-o-sulfonylbenzene imide, 1,3-dibromo-5,5-dimethylhydantoin, 4-carbon tetrabromide, and 1,3,5-tribromo-1,3,5-triazine-2,4,6-trione.

[0009] Optionally, the brominating agent in step (1) is N-bromosuccinimide.

[0010] Optionally, the allyl compound in step (2) is diallylamine.

[0011] The second object of the present invention is to provide an allyl polyphenylene ether resin based on a double-bond polyphenylene ether resin obtained by the preparation method as described above.

[0012] The third object of the present invention is to provide a method for preparing a flexible low dielectric material, which comprises the following steps: fully dissolving the allyl polyphenylene ether resin obtained by the preparation method of any one of claims 1 to 6 and tetrahydrofuran in a mass ratio of 1: (3 to 5), adding the allyl polyphenylene ether resin, dithiol, and photoinitiator in a molar ratio of 1: (5 to 8): (0.01 to 0.03), reacting under ultraviolet light conditions at room temperature for 0.5 to 1 hour to obtain a solvent-based mixture; desolventizing the solvent-based mixture obtained in step (1), and curing it at 60 to 90° C. for 6 to 12 hours to obtain the flexible low dielectric material.

[0013] Optionally, the dithiol is at least one of 1,4-butanedithiol, 1,5-pentanedithiol, 1,6-hexanedithiol, 1,8-octanedithiol, 1,10-decanedithiol, 1,11-undecanedithiol, 1,16-hexadecanedithiol, and polyethylene glycol dithiol.

[0014] Optionally, the photoinitiator is at least one of (2,4,6-trimethylbenzoyl)diphenylphosphine oxide, 2-hydroxy-2-methyl-1-phenyl-1-propanone, and 1-hydroxycyclohexylphenyl ketone.

[0015] A fourth object of the present invention is to provide a flexible low dielectric material obtained by the preparation method as described above.

[0016] The beneficial results of the present invention are as follows:

[0017] The preparation method of the invention can prepare allyl polyphenylene ether resin with excellent performance. The preparation method is simple, the raw materials are easy to obtain, the preparation cycle is short, and the low dielectric performance of the cured flexible material is stable. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is the molecular structure of the allyl polyphenylene ether resin ALPPO in Example 1.

[0019] Figure 2 This is the infrared spectrum of the allyl polyphenylene ether resin ALPPO of Example 1.

[0020] Figure 3 Example 1 Allyl polyphenylene ether resin ALPPO 1 H-NMR.

[0021] Figure 4Graph showing the relationship between the dielectric constant, dielectric loss and frequency of the flexible low dielectric material in Example 1.

[0022] Figure 5 This is the DMA diagram of the flexible low dielectric material in Example 1. DETAILED DESCRIPTION

[0023] In order to make the above-mentioned objects, features and advantages of the invention more obvious and easy to understand, the specific embodiments of the invention are described in detail below.

[0024] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0025] The preparation method of the allyl polyphenylene ether resin according to the present invention comprises the following steps: (1) using polyphenylene ether to react with a brominating agent to obtain brominated polyphenylene ether; (2) using brominated polyphenylene ether to react with an allyl compound to obtain an allyl polyphenylene ether resin.

[0026] In step (1), polyphenylene ether and tetrahydrofuran are dissolved in a mass ratio of 1:(3-5) by a solvent method, and after sufficient dissolution, polyphenylene ether, a brominating agent, and dibenzoyl peroxide are added in a molar ratio of 1:(20-30):(0.2-0.5) to react, and the reaction temperature is maintained at 70-80° C. The reaction is carried out under the protection of high-purity nitrogen for 2 hours, and then cooled to room temperature and washed with anhydrous methanol, and the precipitate is separated to obtain a precipitate, which is vacuum dried, washed and dried 3-4 times, and finally vacuum dried to obtain a solid brominated polyphenylene ether resin.

[0027] In step (2), the brominated polyphenylene ether prepared according to step (1) and tetrahydrofuran are dissolved in a mass ratio of 1:(3-5), and after sufficient dissolution, the brominated polyphenylene ether, the allyl compound and potassium carbonate are added in a molar ratio of 1:(10-20):(3-5) for reaction, the reaction temperature is maintained at 45-50°C, the reaction is carried out under the protection of high-purity nitrogen for 8 hours, and then cooled to room temperature, anhydrous methanol is added for washing, and the precipitate is separated to obtain a precipitate, which is vacuum dried, and the washing and drying are repeated 3-4 times, and finally vacuum dried to obtain a solid allyl polyphenylene ether resin (ALPPO).

[0028] In step (1), the brominating agent may be at least one of N-bromosuccinimide, N-bromo-o-sulfonylbenzene imide, 1,3-dibromo-5,5-dimethylhydantoin, 4-carbon tetrabromide, and 1,3,5-tribromo-1,3,5-triazine-2,4,6-trione. The brominating agent is preferably N-bromosuccinimide.

[0029] In step (2), the allyl compound is preferably diallylamine.

[0030] The allyl polyphenylene ether resin with a high allyl content prepared according to the above preparation method can be applied to the field of low dielectric materials.

[0031] The preparation method of the flexible low dielectric material according to the present invention comprises the following steps: (1) fully dissolving the allyl polyphenylene ether resin and tetrahydrofuran prepared by the above preparation method in a mass ratio of 1:(3-5), adding the allyl polyphenylene ether resin, dithiol and photoinitiator in a molar ratio of 1:(5-8):(0.01-0.03), reacting under ultraviolet light conditions at room temperature for 0.5-1h to obtain a solvent-based mixture; (2) desolventizing the solvent-based mixture obtained in step (1), and curing it at 60-90°C for 6-12 hours to obtain the flexible low dielectric material.

[0032] The dithiol is at least one of 1,4-butanedithiol, 1,5-pentanedithiol, 1,6-hexanedithiol, 1,8-octanedithiol, 1,10-decanedithiol, 1,11-undecanedithiol, 1,16-hexadecanedithiol, and polyethylene glycol dithiol. The dithiol is preferably an alkane chain dithiol, more preferably 1,10-decanedithiol.

[0033] The photoinitiator is at least one of (2,4,6-trimethylbenzoyl) diphenylphosphine oxide, 2-hydroxy-2-methyl-1-phenyl-1-propanone, and 1-hydroxycyclohexyl phenyl ketone. The photoinitiator is preferably (2,4,6-trimethylbenzoyl) diphenylphosphine oxide.

[0034] The flexible low-dielectric material prepared according to the above preparation method has excellent comprehensive properties.

[0035] The allyl polyphenylene ether resin and its preparation method, the flexible low dielectric material and its preparation method of the present invention are specifically described below by examples. Main raw materials and equipment used: Unless otherwise specified, the raw materials and equipment of each embodiment and comparative example are the same; materials without specifying specific models or types are from the same common models purchased on the market, and no specific restrictions are made.

[0036] Example 1

[0037] (1) After fully dissolving 10 g of polyphenylene ether and 50 g of tetrahydrofuran in a 500 ml three-necked flask, 10 g of polyphenylene ether, 26 g of N-bromosuccinimide and 0.5 g of dibenzoyl peroxide were added to react. The reaction temperature was maintained at 70-80° C. The reaction was carried out under the protection of high-purity nitrogen for 2 h. After cooling to room temperature, anhydrous methanol was added for washing. The precipitate was separated and vacuum dried. The washing was repeated 3-4 times. Finally, the solid brominated polyphenylene ether resin was obtained by vacuum drying.

[0038] (2) After fully dissolving 10 g of brominated polyphenylene ether and 50 g of tetrahydrofuran in a 500 ml three-necked flask, add 10 g of brominated polyphenylene ether, 7 g of diallylamine and 2.4 g of potassium carbonate to react. The reaction temperature is maintained at 45-50°C. The reaction is carried out under the protection of high-purity nitrogen for 8 hours. After cooling to room temperature, anhydrous methanol is added for washing. The precipitate is separated and vacuum dried. The washing is repeated 3-4 times. Finally, vacuum drying is performed to obtain solid allyl polyphenylene ether resin (ALPPO). The molecular structure of the reaction product is shown in Figure 1 , where m≥0, n≥0, x≥0, y≥0, the IR and NMR spectra of the reactant PPO and the product ALPPO are shown in Figure 2 and Figure 3 .

[0039] (3) Add 5g of allyl polyphenylene ether resin to a 100ml beaker, and then add 15g of tetrahydrofuran to fully dissolve. Then add 5g of allyl polyphenylene ether, 3g of 1,10-decanedithiol (DCD), and 0.01g of (2,4,6-trimethylbenzoyl) diphenylphosphine oxide to react under ultraviolet light at room temperature for 0.5h. The obtained solvent-based mixture is placed in a mold of a specific shape and baked at 80°C for 10h. After the solvent is fully volatilized and solidified, the temperature is lowered to obtain the final flexible film material.

[0040] The material obtained by the above method was measured by Agilent 4294A instrument. 3 The dielectric properties of the sample were tested and the dielectric constant of the material was 3.14 at 25°C and 1MHz. Figure 4 The dumbbell-shaped specimen was subjected to a bulk tensile test using a universal material testing machine, and the tensile strength of the material was 7.4 MPa and the elongation at break was 18% at 25°C and a tensile rate of 5 mm / min, indicating good mechanical strength and flexibility.

[0041] in, Figure 1 It is the molecular structure of allyl polyphenylene ether resin.

[0042] Figure 2 Medium 3070cm -1 The characteristic peak of CH stretching vibration of allylic unsaturated bond is near 1637cm -1 The C=C characteristic peak is near 919cm -1 The peak near is the characteristic peak of CH bending vibration of allylic unsaturated bond.

[0043] Figure 5 The DMA test results of the material show that the glass transition temperature Tg is 56.5°C and the storage modulus at 25°C is 390 MPa.

[0044] It can be seen from the above test results that the flexible low dielectric material prepared in Example 1 has excellent comprehensive performance.

[0045] Example 2

[0046] (1) According to step (1) of Example 1, except for 10 g of polyphenylene ether, 22 g of N-bromosuccinimide and 0.5 g of dibenzoyl peroxide, the other methods are the same as step (1) of Example 1 to obtain brominated polyphenylene ether.

[0047] (2) According to step (2) of Example 1, except for 10 g of brominated polyphenylene ether, 5 g of diallylamine and 2.4 g of potassium carbonate, the other methods are the same as step (2) of Example 1 to obtain allyl polyphenylene ether.

[0048] (3) According to step (3) of Example 1, except for 5 g of allyl polyphenylene ether, 2.8 g of 1,6-hexanedithiol, and 0.01 g of (2,4,6-trimethylbenzoyl)diphenylphosphine oxide, the other methods are the same as step (3) of Example 1. The final flexible film material is obtained.

[0049] The material obtained by the above method was tested for dielectric properties, and the dielectric constant of the material at 25°C and 1 MHz was 3.23, the tensile strength was 8.8 MPa, and the elongation at break was 16%, and the material had good flexibility and low dielectric properties.

[0050] Example 3

[0051] (1) According to step (1) of Example 1, except for 10 g of polyphenylene ether, 25 g of N-bromosuccinimide and 0.5 g of dibenzoyl peroxide, the other methods are the same as step (1) of Example 1 to obtain brominated polyphenylene ether.

[0052] (2) According to step (2) of Example 1, except for 10 g of brominated polyphenylene ether, 6 g of diallylamine and 2.4 g of potassium carbonate, the other methods are the same as step (2) of Example 1 to obtain allyl polyphenylene ether.

[0053] (3) According to step (3) of Example 1, except for 5 g of allyl polyphenylene ether, 4 g of 1,16-hexadecanedithiol, and 0.01 g of 2-hydroxy-2-methyl-1-phenyl-1-propanone, the other methods are the same as step (3) of Example 1. The final flexible film material is obtained.

[0054] The material obtained by the above method was tested for dielectric properties, and the dielectric constant of the material at 25°C and 1MHz was 3.03, the tensile strength was 5.5MPa, and the elongation at break was 21%, and the material had good flexibility and low dielectric properties.

Claims

1. A method for preparing an allyl polyphenylene ether resin, characterized in that: The following steps are involved: (1) using polyphenylene ether to react with a brominating agent to obtain brominated polyphenylene ether; (2) Allyl polyphenylene ether resin is obtained by reacting brominated polyphenylene ether with an allyl compound.

2. The method for preparing the allyl polyphenylene ether resin according to claim 1, characterized in that: In step (1), polyphenylene ether and tetrahydrofuran are dissolved in a mass ratio of 1:(3-5) by a solvent method, and after sufficient dissolution, polyphenylene ether, a brominating agent, and dibenzoyl peroxide are added in a molar ratio of 1:(20-30):(0.2-0.5) to react, and the reaction temperature is maintained at 70-80° C. The reaction is carried out under the protection of high-purity nitrogen for 2 hours, and then cooled to room temperature and washed with anhydrous methanol, and the precipitate is separated to obtain a precipitate, which is vacuum dried, washed and dried 3-4 times, and finally vacuum dried to obtain a solid brominated polyphenylene ether resin.

3. The method for preparing the allyl polyphenylene ether resin according to claim 1, characterized in that: In step (2), the brominated polyphenylene ether prepared according to step (1) and tetrahydrofuran are dissolved in a mass ratio of 1:(3-5), and after sufficient dissolution, the brominated polyphenylene ether, the allyl compound and potassium carbonate are added in a molar ratio of 1:(10-20):(3-5) for reaction, the reaction temperature is maintained at 45-50°C, the reaction is carried out under the protection of high-purity nitrogen for 8 hours, and then cooled to room temperature, anhydrous methanol is added for washing, and the precipitate is separated to obtain a precipitate, which is vacuum dried, and the washing and drying are repeated 3-4 times, and finally vacuum dried to obtain a solid allyl polyphenylene ether resin (ALPPO).

4. The method for preparing the allyl polyphenylene ether resin according to claim 2, characterized in that: In step (1), the brominating agent is at least one of N-bromosuccinimide, N-bromo-o-sulfonylbenzene imide, 1,3-dibromo-5,5-dimethylhydantoin, 4-carbon tetrabromide, and 1,3,5-tribromo-1,3,5-triazine-2,4,6-trione.

5. The method for preparing allyl polyphenylene ether resin according to claim 4, characterized in that: The brominating agent in step (1) is N-bromosuccinimide.

6. The method for preparing allyl polyphenylene ether resin according to claim 3, characterized in that: The allyl compound in step (2) is diallylamine.

7. An allyl polyphenylene ether resin based on a double-bond polyphenylene ether resin obtained by the preparation method according to any one of claims 1 to 6.

8. A method for preparing a flexible low dielectric material, characterized in that: The following steps are involved: (1) After fully dissolving the allyl polyphenylene ether resin obtained by the preparation method of any one of claims 1 to 6 and tetrahydrofuran in a mass ratio of 1:(3-5), adding the allyl polyphenylene ether resin, dithiol, and photoinitiator in a molar ratio of 1:(5-8):(0.01-0.03), reacting under ultraviolet light at room temperature for 0.5-1h to obtain a solvent-based mixture; (2) Desolventizing the solvent-based mixture obtained in step (1), and curing it at 60 to 90° C. for 6 to 12 hours to obtain the flexible low-dielectric material.

9. The method for preparing a flexible low dielectric material according to claim 8, characterized in that: The dithiol is at least one of 1,4-butanedithiol, 1,5-pentanedithiol, 1,6-hexanedithiol, 1,8-octanedithiol, 1,10-decanedithiol, 1,11-undecanedithiol, 1,16-hexadecanedithiol and polyethylene glycol dithiol.

10. The method for preparing a flexible low dielectric material according to claim 8, characterized in that: The photoinitiator is at least one of (2,4,6-trimethylbenzoyl)diphenylphosphine oxide, 2-hydroxy-2-methyl-1-phenyl-1-propanone, and 1-hydroxycyclohexylphenyl ketone.

Citation Information

Patent Citations

  • Polyphenyl ether-based composite material with low dielectric constant and low dielectric loss and preparation method thereof

    CN115725167A

  • Preparation method of modified low-molecular-weight bifunctional polyphenyl ether oligomer with vinyl-terminated polyphenyl ether

    CN117487155A

  • Method for preparing allylation hyperbranched polyphenylene oxide

    CN101717503A

  • Polyphenyl ether-polyorganosiloxane photo-crosslinking thin film based on graft copolymer and preparation method of polyphenyl ether-polyorganosiloxane photo-crosslinking thin film

    CN108530659A

  • Polyphenyl ether-polysiloxane photo-crosslinking damping material and preparation method thereof

    CN108641337A

Cited By

  • Substituted polyphenylene ether, amino group-containing polyphenylene ether, and thermosetting polyphenylene ether

    WO2026070890A1