High-strength fire-resistant cable and preparation process thereof

By using modified molybdenum selenide carbon nanotubes and polyphosphazene in the cable, combined with high-strength sheathing material, the problem of insufficient fire resistance of the cable in fire and high temperature environments is solved, and the problem of further fire resistance of the cable is achieved High fire resistance and mechanical properties improve the safety of the building.

CN119019788AInactive Publication Date: 2024-11-26JIANGSU DONGXU CABLE CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411518563.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-29
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing cables are insufficient in case of sudden fires, such as fire, resulting in interruption of power transmission, affecting the safety of the building and property losses, and are prone to failure in high temperature environments.

Method used

A cable consisting of a conductive core, an insulating layer and a high-strength refractory sheath, the sheathing materials include ethylene propylene ternary rubber, fluoropolyphosphazene, white carbon black, zinc oxide, etc., and the carbon nano-molybdenum selenide is modified. The combination of tube and polyphosphazene forms antioxidant flame retardant, improving the refractory and mechanical properties of the cable.

Benefits of technology

It significantly improves the refractory and mechanical properties of the cable, extends the power transmission time, remains stable in high temperature environments, and improves the safety of the building.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of fire-resistant cables, and discloses a high-strength fire-resistant cable and a preparation technology thereof.The high-strength fire-resistant cable is provided with a conductive core body, an insulating layer and a high-strength fire-resistant sheath; the insulating layer is coated on the outer surface of the conductive core body, and the high-strength fire-resistant sheath is coated on the outer surface of the insulating layer; the high-strength fire-resistant sheath is prepared from the following raw materials: ethylene propylene diene monomer, fluorinated polyphosphazene, white carbon black, zinc oxide, stearic acid, trichloroethyl phosphate, triallyl isocyanurate, phenolic resin, an anti-aging agent, an antioxidant flame retardant, sulfur and dicumyl peroxide. The raw material composition of the conductive core body comprises copper wires, the diameter of the cross section of the conductive core body is 1.2-2mm, and the number of twisted copper wires is 4-6. The raw material composition of the insulating layer comprises a crosslinked polyethylene insulating material, and the thickness of the insulating layer is 0.7-1.2 mm. And the thickness of the high-strength fire-resistant sheath is 3.4 to 8 mm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fire-resistant cables, in particular to a high-strength fire-resistant cable and a preparation process thereof. Background Art

[0002] With the rapid development of social economy and the acceleration of urbanization, the demand for electricity is increasing. As a key component of power transmission, cables are increasingly used in various types of buildings, infrastructure and industries. Especially in large-scale public places such as shopping malls, hospitals, theaters, subways, etc., cables not only need to carry daily power transmission, but also need to have high safety performance. However, due to the limitations of materials and structures, cables are prone to failure in emergencies such as fires, becoming one of the important reasons for the spread of fires.

[0003] Statistics show that fires caused by wires and cables account for a large proportion of all types of fire accidents. When a fire occurs, the fire resistance of traditional cables is insufficient, and power transmission is often interrupted in a short period of time due to high temperature or combustion, which directly affects the normal operation of key systems such as elevators, lighting, and fire-fighting equipment in buildings, thereby exacerbating casualties and property losses caused by fires. In addition, the surface temperature of cables exposed to high temperature environments is easily too high due to sunlight, further affecting the life and safety of the cables.

[0004] Although the existing fire-resistant cables have improved their fire resistance to a certain extent, their fire resistance time and stability in high temperature environments are still insufficient, especially under extreme conditions, the cables are still prone to failure. Therefore, it is particularly important to develop a high-strength, high-temperature resistant and fire-resistant cable to meet the high standards required by modern society for cables in dangerous situations such as fires. This new type of cable can maintain the power transmission function for a long time when a fire occurs, providing sufficient time for personnel evacuation and firefighting, greatly improving the overall safety of the building. Summary of the invention

[0005] The object of the present invention is to provide a high-strength fire-resistant cable and a preparation process thereof to solve the problems raised in the above background technology.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions: A high-strength fire-resistant cable, comprising a conductive core, an insulating layer and a high-strength fire-resistant sheath; the insulating layer is coated on the outer surface of the conductive core, and the raw materials of the high-strength fire-resistant sheath include the following parts by weight: 80-100 parts of EPDM rubber, 5-20 parts of fluoropolyphosphazene, 20-30 parts of white carbon black, 5-10 parts of zinc oxide, 1-1.5 parts of stearic acid, 1.5-3 parts of trichloroethyl phosphate, 1.5-2 parts of triallyl isocyanurate, 10-15 parts of phenolic resin, 3-5 parts of antioxidant, 30-40 parts of antioxidant flame retardant, 1-1.5 parts of sulfur, and 1-2 parts of dicumyl peroxide.

[0007] Furthermore, the preparation method of the antioxidant flame retardant comprises the following steps: ultrasonically dispersing the modified molybdenum selenide carbon nanotubes in tetrahydrofuran, adding terminal allyl substituted polyphosphazene and triethylamine under a nitrogen atmosphere, stirring at room temperature for 24-26 hours, filtering, washing, and drying to obtain the antioxidant flame retardant; In the antioxidant flame retardant, the mass ratio of modified molybdenum selenide carbon nanotubes: terminal allyl substituted polyphosphazene: triethylamine is 1:3.5:6.

[0008] Furthermore, the conductive core material composition includes copper wire, the conductive core cross-sectional diameter is 1.2-2 mm, and the number of twisted copper wires is 4-6.

[0009] Furthermore, the raw material composition of the insulation layer includes cross-linked polyethylene insulation material, and the thickness of the insulation layer is 0.7-1.2 mm.

[0010] Furthermore, the high-strength fire-resistant sheath has a thickness of 3.4-8 mm.

[0011] Furthermore, the preparation method of the terminal allyl substituted polyphosphazene comprises the following steps: step (1): adding hexachlorocyclotriphosphazene, aminosulfonic acid, calcium sulfate dihydrate, and 1,2,4-trichlorobenzene into a reaction container, heating to 190-192° C. for reaction for 10-15 min under a nitrogen atmosphere, heating to 208-210° C. for reaction until the system becomes viscous and small bubbles appear, filtering while hot, and washing the filtrate with petroleum ether to obtain the polyphosphazene; Step (2): under ice bath conditions and nitrogen atmosphere, add 2-aminoethyl-5(6)-methoxybenzimidazole, triethylamine and diethylene glycol dimethyl ether to a reaction container, add polyphosphazene under ice bath conditions, react at room temperature for 48-50 hours, heat to 110-115° C. for 3-3.5 hours, filter, wash with petroleum ether, and dry to obtain substituted polyphosphazene; add substituted polyphosphazene to dichloromethane, add boron tribromide, and react at room temperature for 48-50 hours to obtain terminal methoxy substituted polyphosphazene; add terminal methoxy substituted polyphosphazene, allyl bromide and potassium carbonate to acetone, heat to reflux for 16-18 hours, distill under reduced pressure, wash, and dry to obtain terminal allyl substituted polyphosphazene; Furthermore, in the polyphosphazene, the mass ratio of hexachlorocyclotriphosphazene:aminosulfonic acid:calcium sulfate dihydrate is 1:0.1:0.01; Furthermore, in the substituted polyphosphazene, the molar ratio of polyphosphazene: 2-aminoethyl-5(6)-methoxybenzimidazole: triethylamine is 1:4:4; in the terminal methoxy-substituted polyphosphazene, the molar ratio of substituted polyphosphazene: boron tribromide is 1:7; in the terminal allyl-substituted polyphosphazene, the molar ratio of terminal methoxy-substituted polyphosphazene: allyl bromide: potassium carbonate is 1:9:6.

[0012] Furthermore, the method for preparing the modified molybdenum selenide carbon nanotubes comprises the following steps: Dispersing molybdenum trioxide and selenium dioxide in an octylamine ethanol mixed solution, stirring evenly, heating to 190-195°C for reaction for 24-26 hours, filtering, washing, and vacuum drying to obtain molybdenum selenide carbon nanotubes; ultrasonically dispersing molybdenum selenide carbon nanotubes in an ethanol solution, adding 3-aminopropyltriethoxysilane, heating to 50-55°C for reaction for 12-14 hours, filtering, washing, and drying to obtain modified molybdenum selenide carbon nanotubes; Furthermore, in the molybdenum selenide carbon nanotubes, the mass ratio of molybdenum trioxide: selenium dioxide is 0.68:1.04; in the modified molybdenum selenide carbon nanotubes, the mass ratio of molybdenum selenide carbon nanotubes: 3-aminopropyltriethoxysilane is 1:5.

[0013] Furthermore, the preparation method of the fluorinated polyphosphazene comprises the following steps: Adding sodium metal to tetrahydrofuran, adding undecenol under ice bath conditions and nitrogen atmosphere, heating, condensing and refluxing until the sodium metal disappears, to obtain nucleophilic reagent A; adding sodium metal to tetrahydrofuran, adding trifluoroethanol and octafluoropentanol under ice bath conditions and nitrogen atmosphere, heating, condensing and refluxing until the sodium metal disappears, to obtain nucleophilic reagent B; adding a xylene solution of polyphosphazene to nucleophilic reagent B under ice bath conditions, reacting for 2-2.5h, adding nucleophilic reagent A, reacting for 1-1.5h, removing the ice bath, continuing the reaction at room temperature for 12-13h, washing with petroleum ether and deionized water, dissolving in tetrahydrofuran, deionizing washing, and vacuum drying to obtain fluoropolyphosphazene; Furthermore, in the fluorinated polyphosphazene, the mass ratio of polyphosphazene: nucleophile A: nucleophile B is 1:0.7:0.8; and in the nucleophile B, the molar ratio of trifluoroethanol: octafluoropentanol is 4:6.

[0014] Furthermore, the preparation method of the polyphosphazene is the same as the preparation method of the polyphosphazene in the antioxidant flame retardant.

[0015] A preparation process of a high-strength fire-resistant cable comprises the following steps: S1: adding EPDM rubber and fluoropolyphosphazene to an internal mixer and plasticizing for 10-15 minutes to obtain plasticized rubber A and plasticized rubber B; adding plasticized rubber A and plasticized rubber B to a mixer, adding white carbon black, zinc oxide, stearic acid, trichloroethyl phosphate, triallyl isocyanurate, phenolic resin, and antioxidant flame retardant in sequence and mixing for 10-20 minutes, adding sulfur and dicumyl peroxide and mixing for 10-20 minutes, thinning, standing, hot pressing and vulcanizing at 140-142°C, and hot air vulcanizing at 149-151°C, respectively, to obtain a high-strength fire-resistant sheath; S2: The conductor metal is drawn, annealed, and twisted to obtain a conductive core; a cross-linked polyethylene insulating material is extruded on the surface of the conductive core to obtain an insulating layer, and a high-strength fire-resistant sheath is extruded on the surface of the insulating layer. After cooling and solidification, the sheath is cut to obtain a high-strength fire-resistant cable.

[0016] Compared with the prior art, the beneficial effects achieved by the present invention are: The invention uses the prepared molybdenum selenide carbon nanotubes as a matrix material, performs aminosiloxane modification treatment on the matrix material, loads a large number of amine active groups on the surface of the matrix material, and then undergoes a substitution reaction with the chlorine on the polyphosphazene to prepare an antioxidant flame retardant. On the one hand, acidic substances such as phosphoric acid and metaphosphoric acid generated by thermal decomposition of the polyphosphazene form a thin film on the matrix surface to prevent the penetration of oxygen and combustible gas, help the matrix to dehydrate and form a carbon layer, and also generate non-combustible gas to help the formation of an expanded carbon layer, dilute the combustible gas and oxygen, generate free radicals to quench the active free radicals in the combustion area, delay or inhibit the combustion reaction, and improve the fire resistance and flame retardancy of the cable. On the other hand, the use of molybdenum selenide carbon nanotubes as transition metal compounds has a catalytic carbonization effect, which can promote the formation of high-quality, strong and dense carbon layer in the cable during the thermal combustion process, thereby improving the fire resistance and flame retardancy of the cable; at the same time, the polyphosphazene containing terminal allyl structure substituted and grafted on its surface can promote the vulcanization performance of EPDM rubber, improve the compatibility of antioxidant flame retardants in EPDM rubber, serve as the physical cross-linking point of the rubber matrix and form a pinning effect with the polymer interface to form a stable composite structure, thereby improving the mechanical properties of the cable.

[0017] On this basis, the present invention carries out substitution modification on the polyphosphazene, and controls the amount of substances added in the substitution reaction process to control the substitution rate of active chlorine in the polyphosphazene molecular chain segment, so that the polyphosphazene can contain a large number of additional functional groups while meeting the requirements of coating the surface of molybdenum selenide carbon nanotubes, thereby achieving the purpose of the synergistic effect between the substances. 2-Aminoethyl-5(6)-methoxybenzimidazole is selected as the substitution modification group, the terminal methoxybenzimidazole group is grafted on the surface of the polyphosphazene, and finally the terminal methoxy group is reduced and then grafted with an allyl group to obtain a benzimidazole group with a terminal allyl structure; on the one hand, the active double bond structure is introduced into the antioxidant flame retardant, which has the function of an auxiliary crosslinking agent, can improve the crosslinking density of the rubber matrix, enhance the compatibility between the antioxidant flame retardant and the rubber matrix, and avoid the problem of reduced crosslinking reaction of rubber macromolecules and reduced vulcanization rate caused by the addition of traditional flame retardants such as peroxides; on the other hand, the benzimidazole antioxidant structure is introduced into the rubber matrix. With the help of the terminal allyl group, the migration of traditional antioxidants in the rubber matrix, reduced matrix crosslinking density, and uneven crosslinking network can be effectively avoided, which greatly improves the thermal stability of the cable during high temperature and thermal oxidation aging, and improves the fire resistance and mechanical properties of the cable.

[0018] In order to further improve the mechanical properties and fire resistance of the cable, the present invention introduces trifluoroethanol, octafluoropentanol and undecenol on the basis of homemade polyphosphazene, prepares a fluorinated polyphosphazene with a phosphorus-nitrogen main chain and a side group structure containing an olefin bond and a carbon-fluorine bond, and adjusts the vulcanization process, adopts a secondary vulcanization method of hot pressing vulcanization and hot air vulcanization, and further improves the mechanical properties of the high-strength fire-resistant sheath on the basis of the previous one. Due to the smaller steric hindrance of the fluorinated alkoxy side chain group of the fluorinated polyphosphazene, there is a strong mutual entanglement between the entire molecular chain, and in a hot pressing vulcanization process, chemical crosslinking is generated, and the molecular chain is not easy to move under high pressure to generate internal stress, resulting in a decrease in the mechanical properties of the rubber. Through the introduction of the second stage hot air vulcanization, the volatilization of small molecular byproducts can be helped, and the tensile strength of the rubber is improved on the basis of ensuring the similar elongation at break of the rubber. The high bond energy CF bond in the molecular structure of fluorinated polyphosphazene and the dπ-pπ conjugated effect composed of alternating single and double bonds of phosphorus and nitrogen in the main chain of polyphosphazene in the fluorinated polyphosphazene and antioxidant flame retardant have a high structural stability, which further improves the high temperature resistance and fire resistance of the rubber. DETAILED DESCRIPTION

[0019] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] In the following examples, graphene oxide was purchased from Changzhou Sixth Element Material Technology Co., Ltd.; polytetramethylene ether glycol with a molecular weight of 1000 was purchased from Henan Tianfu Chemical Co., Ltd.; the cross-linked polyethylene insulation material model is XLPE insulation material, purchased from Jiangsu Dewei New Materials Co., Ltd.; the remaining raw materials are commercially available.

[0021] The preparation method of the antioxidant flame retardant comprises the following steps: Step (1): 10 g of hexachlorocyclotriphosphazene, 1 g of aminosulfonic acid, 0.1 g of calcium sulfate dihydrate, and 10 mL of 1,2,4-trichlorobenzene are added to a reaction container, heated to 190° C. for reaction for 10 min under a nitrogen atmosphere, and then heated to 208° C. for reaction until the system becomes viscous and small bubbles appear, and filtered while hot, and the filtrate is washed with petroleum ether to obtain a polyphosphazene; Step (2): under ice bath conditions and nitrogen atmosphere, 4 mmol 2-aminoethyl-5(6)-methoxybenzimidazole, 4 mmol triethylamine and 50 mL diethylene glycol dimethyl ether are added to a reaction container, 1 mmol polyphosphazene is added under ice bath conditions, the reaction is carried out at room temperature for 48 h, the reaction is heated to 110° C. for 3 h, the reaction is filtered, the reaction is washed with petroleum ether and dried to obtain a substituted polyphosphazene; 1 mmol substituted polyphosphazene is added to dichloromethane, 7 mmol boron tribromide is added and the reaction is carried out at room temperature for 48 h to obtain a terminal methoxy substituted polyphosphazene; 1 mmol terminal methoxy substituted polyphosphazene, 9 mmol allyl bromide and 6 mmol potassium carbonate are added to acetone, the reaction is heated under reflux for 16 h, the reaction is carried out under reduced pressure distillation, the reaction is washed and dried to obtain a terminal allyl substituted polyphosphazene; Step (3): ultrasonically disperse 1 g of modified molybdenum selenide carbon nanotubes in tetrahydrofuran, add 3.5 g of terminal allyl-substituted polyphosphazene and 6 g of triethylamine under a nitrogen atmosphere, stir at room temperature for 24 h, filter, wash, and dry to obtain an antioxidant flame retardant.

[0022] The method for preparing the modified molybdenum selenide carbon nanotubes comprises the following steps: 0.68g of molybdenum trioxide and 1.04g of selenium dioxide were dispersed in 20mL of a 1:1 volume ratio octylamine ethanol mixed solution, stirred evenly, heated to 190°C for reaction for 24h, filtered, washed, and vacuum dried to obtain molybdenum selenide carbon nanotubes; 1g of molybdenum selenide carbon nanotubes was ultrasonically dispersed in an ethanol solution, 5g of 3-aminopropyltriethoxysilane was added, heated to 50°C for reaction for 12h, filtered, washed, and dried to obtain modified molybdenum selenide carbon nanotubes.

[0023] The preparation method of the fluorinated polyphosphazene comprises the following steps: 1 mol of metallic sodium is added to tetrahydrofuran, and 1 mol of undecenyl alcohol is added under ice bath conditions and nitrogen atmosphere, and the mixture is heated, condensed and refluxed until the metallic sodium disappears to obtain nucleophilic reagent A; 1 mol of metallic sodium is added to tetrahydrofuran, and 0.4 mol of trifluoroethanol and 0.6 mol of octafluoropentanol are added under ice bath conditions and nitrogen atmosphere, and the mixture is heated, condensed and refluxed until the metallic sodium disappears to obtain nucleophilic reagent B; under ice bath conditions, 1 g of a xylene solution of polyphosphazene is added to 0.8 g of nucleophilic reagent B, and the reaction is carried out for 2 h, and 0.7 g of nucleophilic reagent A is added, and the reaction is carried out for 1 h, the ice bath is removed, and the reaction is continued at room temperature for 12 h, and the mixture is washed with petroleum ether and deionized water, dissolved in tetrahydrofuran, washed with deionized water, and dried in vacuum to obtain a fluoropolyphosphazene.

[0024] Embodiment 1: A preparation process of a high-strength fire-resistant cable: S1: 100 parts of EPDM rubber and 5 parts of fluoropolyphosphazene are added to an internal mixer and plasticized for 10 minutes to obtain plasticized rubber A and plasticized rubber B; plasticized rubber A and plasticized rubber B are added to a mixer, and 20 parts of white carbon black, 5 parts of zinc oxide, 1 part of stearic acid, 1.5 parts of trichloroethyl phosphate, 1.5 parts of triallyl isocyanurate, 10 parts of phenolic resin, and 30 parts of antioxidant flame retardant are added in sequence and mixed for 10 minutes, and 1 part of sulfur and 1 part of diisopropylbenzene peroxide are added and mixed for 10 minutes, and the mixture is thinned, allowed to stand, and hot-pressed and vulcanized at 140°C and 15MPa for 30 minutes and hot-air vulcanized at 149°C for 30 minutes to obtain a high-strength fire-resistant sheath; S2: The copper wire is drawn into a diameter of 1.5 mm, annealed, and 4 copper wires are twisted to obtain a conductive core; a cross-linked polyethylene insulating material is extruded on the surface of the conductive core to obtain an insulating layer, and a high-strength fire-resistant sheath is extruded on the surface of the insulating layer. After cooling and solidification, the sheath is cut to obtain a high-strength fire-resistant cable.

[0025] Embodiment 2: A preparation process of a high-strength fire-resistant cable: S1: 100 parts of EPDM rubber and 15 parts of fluoropolyphosphazene are added to an internal mixer and plasticized for 10 minutes to obtain plasticized rubber A and plasticized rubber B; plasticized rubber A and plasticized rubber B are added to a mixer, and 20 parts of white carbon black, 5 parts of zinc oxide, 1 part of stearic acid, 1.5 parts of trichloroethyl phosphate, 1.5 parts of triallyl isocyanurate, 10 parts of phenolic resin, and 30 parts of antioxidant flame retardant are added in sequence and mixed for 10 minutes, and 1 part of sulfur and 1 part of diisopropylbenzene peroxide are added and mixed for 10 minutes, and the mixture is thinned, allowed to stand, and hot-pressed and vulcanized at 140°C and 15MPa for 30 minutes and hot-air vulcanized at 149°C for 30 minutes to obtain a high-strength fire-resistant sheath; S2: The copper wire is drawn into a diameter of 1.5 mm, annealed, and 4 copper wires are twisted to obtain a conductive core; a cross-linked polyethylene insulating material is extruded on the surface of the conductive core to obtain an insulating layer, and a high-strength fire-resistant sheath is extruded on the surface of the insulating layer. After cooling and solidification, the sheath is cut to obtain a high-strength fire-resistant cable.

[0026] Embodiment 3: A preparation process of a high-strength fire-resistant cable: S1: 100 parts of EPDM rubber and 5 parts of fluoropolyphosphazene are added to an internal mixer and plasticized for 10 minutes to obtain plasticized rubber A and plasticized rubber B; plasticized rubber A and plasticized rubber B are added to a mixer, and 20 parts of white carbon black, 5 parts of zinc oxide, 1 part of stearic acid, 1.5 parts of trichloroethyl phosphate, 1.5 parts of triallyl isocyanurate, 10 parts of phenolic resin, and 40 parts of antioxidant flame retardant are added in sequence and mixed for 10 minutes, and 1 part of sulfur and 1 part of diisopropylbenzene peroxide are added and mixed for 10 minutes, and the mixture is thinned and allowed to stand, and hot-pressed and vulcanized at 140°C and 15MPa for 30 minutes and hot-air vulcanized at 149°C for 30 minutes to obtain a high-strength fire-resistant sheath; S2: The copper wire is drawn into a diameter of 1.5 mm, annealed, and 4 copper wires are twisted to obtain a conductive core; a cross-linked polyethylene insulating material is extruded on the surface of the conductive core to obtain an insulating layer, and a high-strength fire-resistant sheath is extruded on the surface of the insulating layer. After cooling and solidification, the sheath is cut to obtain a high-strength fire-resistant cable.

[0027] Embodiment 4: A preparation process of a high-strength fire-resistant cable: S1: 100 parts of EPDM rubber and 15 parts of fluoropolyphosphazene are added to an internal mixer and plasticized for 10 minutes to obtain plasticized rubber A and plasticized rubber B; plasticized rubber A and plasticized rubber B are added to a mixer, and 20 parts of white carbon black, 10 parts of zinc oxide, 1.5 parts of stearic acid, 3 parts of trichloroethyl phosphate, 2 parts of triallyl isocyanurate, 10 parts of phenolic resin, and 40 parts of antioxidant flame retardant are added in sequence and mixed for 10 minutes, and 1.5 parts of sulfur and 2 parts of diisopropylbenzene peroxide are added and mixed for 10 minutes, and then the mixture is thinned and allowed to stand, and hot-pressed and vulcanized at 140°C and 15MPa for 30 minutes and hot-air vulcanized at 149°C for 30 minutes to obtain a high-strength fire-resistant sheath; S2: The copper wire is drawn into a diameter of 1.5 mm, annealed, and 4 copper wires are twisted to obtain a conductive core; a cross-linked polyethylene insulating material is extruded on the surface of the conductive core to obtain an insulating layer, and a high-strength fire-resistant sheath is extruded on the surface of the insulating layer. After cooling and solidification, the sheath is cut to obtain a high-strength fire-resistant cable.

[0028] Comparative Example 1: A preparation process of a high-strength fire-resistant cable: The preparation method of the antioxidant flame retardant comprises the following steps: Step (1): 10 g of hexachlorocyclotriphosphazene, 1 g of aminosulfonic acid, 0.1 g of calcium sulfate dihydrate, and 10 mL of 1,2,4-trichlorobenzene are added to a reaction container, heated to 190° C. for reaction for 10 min under a nitrogen atmosphere, and then heated to 208° C. for reaction until the system becomes viscous and small bubbles appear, and filtered while hot, and the filtrate is washed with petroleum ether to obtain a polyphosphazene; Step (2): under ice bath conditions and nitrogen atmosphere, 4 mmol 2-aminoethyl-5(6)-methoxybenzimidazole, 4 mmol triethylamine and 50 mL diethylene glycol dimethyl ether are added to a reaction container, 1 mmol polyphosphazene is added under ice bath conditions, the reaction is carried out at room temperature for 48 h, the reaction is heated to 110° C. for 3 h, the reaction is filtered, the reaction is washed with petroleum ether and dried to obtain a substituted polyphosphazene; 1 mmol substituted polyphosphazene is added to dichloromethane, 7 mmol boron tribromide is added and the reaction is carried out at room temperature for 48 h to obtain a terminal methoxy substituted polyphosphazene; 1 mmol terminal methoxy substituted polyphosphazene, 9 mmol allyl bromide and 6 mmol potassium carbonate are added to acetone, the reaction is heated under reflux for 16 h, the reaction is carried out under reduced pressure distillation, the reaction is washed and dried to obtain a terminal allyl substituted polyphosphazene; Step (3): ultrasonically disperse 1 g of modified carbon nanotubes in tetrahydrofuran, add 3.5 g of terminal allyl-substituted polyphosphazene and 6 g of triethylamine under a nitrogen atmosphere, stir at room temperature for 24 h, filter, wash, and dry to obtain an antioxidant flame retardant.

[0029] The method for preparing the modified molybdenum selenide carbon nanotubes comprises the following steps: 1 g of carbon nanotubes was ultrasonically dispersed in an ethanol solution, 5 g of 3-aminopropyltriethoxysilane was added, and the solution was heated to 50° C. for reaction for 12 h, filtered, washed, and dried to obtain modified molybdenum selenide carbon nanotubes.

[0030] The remaining steps are the same as those in Example 1.

[0031] Comparative Example 2: A preparation process of a high-strength fire-resistant cable: The preparation method of the antioxidant flame retardant comprises the following steps: Step (1): 10 g of hexachlorocyclotriphosphazene, 1 g of aminosulfonic acid, 0.1 g of calcium sulfate dihydrate, and 10 mL of 1,2,4-trichlorobenzene are added to a reaction container, heated to 190° C. for reaction for 10 min under a nitrogen atmosphere, and then heated to 208° C. for reaction until the system becomes viscous and small bubbles appear, and filtered while hot, and the filtrate is washed with petroleum ether to obtain a polyphosphazene; Step (2): under ice bath conditions and nitrogen atmosphere, 4 mmol eugenol, 4 mmol triethylamine and 50 mL diethylene glycol dimethyl ether are added to a reaction container, 1 mmol polyphosphazene is added under ice bath conditions, the reaction is carried out at room temperature for 48 h, the reaction is heated to 110° C. for 3 h, the reaction is filtered, the reaction is washed with petroleum ether and dried to obtain a substituted polyphosphazene; 1 mmol substituted polyphosphazene is added to dichloromethane, 7 mmol boron tribromide is added and the reaction is carried out at room temperature for 48 h to obtain a terminal methoxy substituted polyphosphazene; 1 mmol terminal methoxy substituted polyphosphazene, 9 mmol allyl bromide and 6 mmol potassium carbonate are added to acetone, the reaction is heated under reflux for 16 h, the reaction is carried out under reduced pressure distillation, the reaction is washed and dried to obtain a terminal allyl substituted polyphosphazene; Step (3): ultrasonically disperse 1 g of modified carbon nanotubes in tetrahydrofuran, add 3.5 g of terminal allyl-substituted polyphosphazene and 6 g of triethylamine under a nitrogen atmosphere, stir at room temperature for 24 h, filter, wash, and dry to obtain an antioxidant flame retardant.

[0032] S1: 100 parts of EPDM rubber and 5 parts of fluoropolyphosphazene are added to an internal mixer and plasticized for 10 minutes to obtain plasticized rubber A and plasticized rubber B; plasticized rubber A and plasticized rubber B are added to a mixer, and 20 parts of white carbon black, 5 parts of zinc oxide, 1 part of stearic acid, 1.5 parts of trichloroethyl phosphate, 1.5 parts of triallyl isocyanurate, 1.5 parts of 2-mercaptobenzimidazole antioxidant, 10 parts of phenolic resin, and 30 parts of antioxidant flame retardant are added in sequence and mixed for 10 minutes, and 1 part of sulfur and 1 part of diisopropylbenzene peroxide are added and mixed for 10 minutes, and then the mixture is thinned, allowed to stand, and hot-pressed and vulcanized at 140°C and 15MPa for 30 minutes and hot-air vulcanized at 149°C for 30 minutes to obtain a high-strength fire-resistant sheath; S2: The copper wire is drawn into a diameter of 1.5 mm, annealed, and 4 copper wires are twisted to obtain a conductive core; a cross-linked polyethylene insulating material is extruded on the surface of the conductive core to obtain an insulating layer, and a high-strength fire-resistant sheath is extruded on the surface of the insulating layer. After cooling and solidification, the sheath is cut to obtain a high-strength fire-resistant cable.

[0033] Comparative Example 3: A preparation process for a high-strength fire-resistant cable: S1: Add 100 parts of EPDM rubber to an internal mixer and plasticize for 10 minutes to obtain plasticized rubber; add the plasticized rubber to a mixer, add 20 parts of white carbon black, 5 parts of zinc oxide, 1 part of stearic acid, 1.5 parts of trichloroethyl phosphate, 1.5 parts of triallyl isocyanurate, 10 parts of phenolic resin, and 30 parts of antioxidant flame retardant in sequence and mix for 10 minutes, add 1 part of sulfur and 1 part of diisopropylbenzene peroxide and mix for 10 minutes, thin through, let stand, and hot press vulcanize at 140°C and 15MPa for 30 minutes and hot air vulcanize at 149°C for 30 minutes to obtain a high-strength fire-resistant sheath; S2: The copper wire is drawn into a diameter of 1.5 mm, annealed, and 4 copper wires are twisted to obtain a conductive core; a cross-linked polyethylene insulating material is extruded on the surface of the conductive core to obtain an insulating layer, and a high-strength fire-resistant sheath is extruded on the surface of the insulating layer. After cooling and solidification, the sheath is cut to obtain a high-strength fire-resistant cable.

[0034] Comparative Example 4: A preparation process for a high-strength fire-resistant cable: S1: 100 parts of EPDM rubber and 5 parts of fluoropolyphosphazene are added to an internal mixer and plasticized for 10 minutes to obtain plasticized rubber A and plasticized rubber B; plasticized rubber A and plasticized rubber B are added to a mixer, and 20 parts of white carbon black, 5 parts of zinc oxide, 1 part of stearic acid, 1.5 parts of trichloroethyl phosphate, 1.5 parts of triallyl isocyanurate, 10 parts of phenolic resin, and 30 parts of antioxidant flame retardant are added in sequence and mixed for 10 minutes, and 1 part of sulfur and 1 part of diisopropylbenzene peroxide are added and mixed for 10 minutes, and then the mixture is thinned, allowed to stand, and hot-pressed and vulcanized at 160°C and 15MPa for 30 minutes to obtain a high-strength fire-resistant sheath; S2: The copper wire is drawn into a diameter of 1.5 mm, annealed, and 4 copper wires are twisted to obtain a conductive core; a cross-linked polyethylene insulating material is extruded on the surface of the conductive core to obtain an insulating layer, and a high-strength fire-resistant sheath is extruded on the surface of the insulating layer. After cooling and solidification, the sheath is cut to obtain a high-strength fire-resistant cable.

[0035] Experiment: Tensile strength test: Mechanical test of high-strength fire-resistant sheath was carried out according to GB / T 528-1998; the tensile rate was 200mm / min and the test temperature was room temperature; Limiting oxygen index test: Test the limiting oxygen index of high-strength fire-resistant sheath according to GB / T 2406.1-2008; Fire resistance test: The cable is placed at 750°C and burned for 90 minutes, and it is recorded whether the cable maintains normal conductivity.

[0036] The experimental data are shown in Table 1 below.

[0037] Table 1 High-strength fire-resistant sheath and cable performance test data

[0038] Conclusion: The cable prepared by the present invention has excellent mechanical properties and fire resistance.

[0039] Comparative Example 1 uses ordinary carbon nanotubes instead of molybdenum selenide carbon nanotubes; the lack of metal compounds to catalyze the formation of the carbon layer leads to reduced fire resistance.

[0040] Comparative Example 2 uses eugenol to replace 2-aminoethyl-5(6)-methoxybenzimidazole, and adds an additional 2-mercaptobenzimidazole antioxidant, which results in reduced compatibility, reduced mechanical properties, and reduced fire resistance.

[0041] Comparative Example 3 does not add fluorinated polyphosphazene, resulting in reduced mechanical properties and fire resistance.

[0042] Comparative Example 4 uses one-stage hot pressing to prepare a high-strength fire-resistant jacket, resulting in reduced mechanical properties.

[0043] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A high-strength fire-resistant cable, characterized in that: The high-strength fire-resistant cable is provided with a conductive core, an insulating layer and a high-strength fire-resistant sheath; The insulating layer is coated on the outer surface of the conductive core, and the high-strength fire-resistant sheath is coated on the outer surface of the insulating layer; The raw material composition of the high-strength fire-resistant sheath includes the following parts by weight: 80-100 parts of EPDM rubber, 5-20 parts of fluoropolyphosphazene, 20-30 parts of white carbon black, 5-10 parts of zinc oxide, 1-1.5 parts of stearic acid, 1.5-3 parts of trichloroethyl phosphate, 1.5-2 parts of triallyl isocyanurate, 10-15 parts of phenolic resin, 3-5 parts of antioxidant, 30-40 parts of antioxidant flame retardant, 1-1.5 parts of sulfur, and 1-2 parts of dicumyl peroxide; The preparation method of the antioxidant flame retardant comprises the following steps: ultrasonically dispersing the modified molybdenum selenide carbon nanotubes in tetrahydrofuran, adding terminal allyl substituted polyphosphazene and triethylamine under a nitrogen atmosphere, stirring at room temperature for 24-26 hours, filtering, washing, and drying to obtain the antioxidant flame retardant; In the antioxidant flame retardant, the mass ratio of modified molybdenum selenide carbon nanotubes: terminal allyl substituted polyphosphazene: triethylamine is 1:3.5:

6.

2. A high-strength fire-resistant cable according to claim 1, characterized in that: The conductive core material comprises copper wire, the conductive core cross-sectional diameter is 1.2-2 mm, and the number of twisted copper wires is 4-6.

3. A high-strength fire-resistant cable according to claim 1, characterized in that: The insulating layer material composition includes cross-linked polyethylene insulating material, and the thickness of the insulating layer is 0.7-1.2 mm.

4. A high-strength fire-resistant cable according to claim 1, characterized in that: The thickness of the high-strength fire-resistant sheath is 3.4-8 mm.

5. A high-strength fire-resistant cable according to claim 1, characterized in that: The preparation method of the terminal allyl substituted polyphosphazene comprises the following steps: step (1): adding hexachlorocyclotriphosphazene, aminosulfonic acid, calcium sulfate dihydrate and 1,2,4-trichlorobenzene into a reaction container, heating to 190-192° C. for reaction for 10-15 min under a nitrogen atmosphere, heating to 208-210° C. for reaction until the system becomes viscous and small bubbles appear, filtering while hot, and washing the filtrate with petroleum ether to obtain the polyphosphazene; Step (2): under ice bath conditions and nitrogen atmosphere, add 2-aminoethyl-5(6)-methoxybenzimidazole, triethylamine and diethylene glycol dimethyl ether to a reaction container, add polyphosphazene under ice bath conditions, react at room temperature for 48-50 hours, heat to 110-115° C. for 3-3.5 hours, filter, wash with petroleum ether, and dry to obtain substituted polyphosphazene; add substituted polyphosphazene to dichloromethane, add boron tribromide, and react at room temperature for 48-50 hours to obtain terminal methoxy substituted polyphosphazene; add terminal methoxy substituted polyphosphazene, allyl bromide and potassium carbonate to acetone, heat to reflux for 16-18 hours, distill under reduced pressure, wash, and dry to obtain terminal allyl substituted polyphosphazene; In the polyphosphazene, the mass ratio of hexachlorocyclotriphosphazene:aminosulfonic acid:calcium sulfate dihydrate is 1:0.1:0.01; In the substituted polyphosphazene, the molar ratio of polyphosphazene: 2-aminoethyl-5(6)-methoxybenzimidazole: triethylamine is 1:4:4; in the terminal methoxy-substituted polyphosphazene, the molar ratio of substituted polyphosphazene: boron tribromide is 1:7; in the terminal allyl-substituted polyphosphazene, the molar ratio of terminal methoxy-substituted polyphosphazene: allyl bromide: potassium carbonate is 1:9:

6.

6. A high-strength fire-resistant cable according to claim 1, characterized in that: The method for preparing the modified molybdenum selenide carbon nanotubes comprises the following steps: Dispersing molybdenum trioxide and selenium dioxide in an octylamine ethanol mixed solution, stirring evenly, heating to 190-195°C for reaction for 24-26 hours, filtering, washing, and vacuum drying to obtain molybdenum selenide carbon nanotubes; ultrasonically dispersing molybdenum selenide carbon nanotubes in an ethanol solution, adding 3-aminopropyltriethoxysilane, heating to 50-55°C for reaction for 12-14 hours, filtering, washing, and drying to obtain modified molybdenum selenide carbon nanotubes; In the molybdenum selenide carbon nanotubes, the mass ratio of molybdenum trioxide to selenium dioxide is 0.68:1.04; in the modified molybdenum selenide carbon nanotubes, the mass ratio of molybdenum selenide carbon nanotubes to 3-aminopropyltriethoxysilane is 1:

5.

7. A high-strength fire-resistant cable according to claim 1, characterized in that: The preparation method of the fluorinated polyphosphazene comprises the following steps: Adding sodium metal to tetrahydrofuran, adding undecenol under ice bath conditions and nitrogen atmosphere, heating, condensing and refluxing until the sodium metal disappears, to obtain nucleophilic reagent A; adding sodium metal to tetrahydrofuran, adding trifluoroethanol and octafluoropentanol under ice bath conditions and nitrogen atmosphere, heating, condensing and refluxing until the sodium metal disappears, to obtain nucleophilic reagent B; adding a xylene solution of polyphosphazene to nucleophilic reagent B under ice bath conditions, reacting for 2-2.5h, adding nucleophilic reagent A, reacting for 1-1.5h, removing the ice bath, continuing the reaction at room temperature for 12-13h, washing with petroleum ether and deionized water, dissolving in tetrahydrofuran, deionizing washing, and vacuum drying to obtain fluoropolyphosphazene; In the fluorinated polyphosphazene, the mass ratio of polyphosphazene: nucleophile A: nucleophile B is 1:0.7:0.8; in the nucleophile B, the molar ratio of trifluoroethanol: octafluoropentanol is 4:

6.

8. A process for preparing a high-strength fire-resistant cable according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: S1: adding EPDM rubber and fluoropolyphosphazene to an internal mixer and plasticizing for 10-15 minutes to obtain plasticized rubber A and plasticized rubber B; adding plasticized rubber A and plasticized rubber B to a mixer, adding white carbon black, zinc oxide, stearic acid, trichloroethyl phosphate, triallyl isocyanurate, phenolic resin and antioxidant flame retardant in sequence and mixing for 10-20 minutes, adding sulfur and dicumyl peroxide and mixing for 10-20 minutes, thinning, standing, hot pressing vulcanizing at 140-142°C and hot air vulcanizing at 149-151°C, respectively, to obtain a high-strength fire-resistant sheath; S2: The conductor metal is drawn, annealed, and twisted to obtain a conductive core; a cross-linked polyethylene insulating material is extruded on the surface of the conductive core to obtain an insulating layer, and a high-strength fire-resistant sheath is extruded on the surface of the insulating layer. After cooling and solidification, the sheath is cut to obtain a high-strength fire-resistant cable.

Citation Information

Patent Citations

  • High-strength heat-resistant cable and preparation method thereof

    CN111499931A

  • Floating type overwater photovoltaic multi-core dynamic submarine cable and preparation method thereof

    CN117747180A

  • Halogen-free flame-retardant aging-resistant cable material and preparation method thereof

    CN118652503A