In-situ molded single-component addition type liquid silicone rubber and preparation method thereof

By using phenyl vinyl MDQ silicone resin and epoxy group tackifier in on-site molding single-component addition-molded liquid silicone rubber, combined with hydrophobic gas-phase white carbon black, the large dimensional change rate and bonding before and after high-temperature curing are solved. The problem of poor performance achieves excellent adhesion and removability to metal substrates, significantly improving mechanical properties and compression rebound properties.

CN119019851AActive Publication Date: 2024-11-26FOSHAN BAFULUO NEW MATERIAL TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411284676.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-26
Estimated Expiration
2044-09-13

AI Technical Summary

Technical Problem

The existing in-situ molded single-component addition-molded liquid silicone rubber has a large dimensional change rate before and after high-temperature curing, and has poor adhesive performance, making it difficult to achieve lossless disassembly and rework, and has poor extrusion and compatibility problems.

Method used

Use phenylvinyl MDQ silicone resin to conduct hydrogen silicification addition reaction with silicon hydrogen bonded silicone polymer, design tackifier with epoxy and benzene ring groups and epoxy group grafted polymethyl hydrogen Silicone thixotropic agent promotes cross-linking vulcanization through catalysts, improves cohesive energy density and heat resistance, and improves mechanical properties through hydrophobic gas-phase white carbon black.

Benefits of technology

It achieves good adhesion to metal substrates, has small dimensional change rate after high-temperature curing, excellent compression elasticity and removability, significantly improves shear strength and tensile strength, and has low compression permanent deformation rate, avoids seepage Oil and adhesion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019851A_ABST
    Figure CN119019851A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of liquid silicone rubber, and particularly discloses in-situ molded single-component addition type liquid silicone rubber and a preparation method thereof. Vinyl silicone oil, nano silicon dioxide and silicon resin are kneaded to prepare base rubber, the base rubber is matched with additives such as a cross-linking agent, a tackifier, a thixotropic agent, an inhibitor and a platinum catalyst according to a proper proportion, and defoaming is performed to prepare the silicon rubber, the preparation process is simple, and the prepared silicon rubber product has the advantages of single-component packaging and convenience and simplicity in use; and no small molecules are released in the curing process, so that the coating is efficient and environment-friendly. The silicone rubber cured at high temperature has excellent mechanical properties (the tensile strength is greater than 5MP, the elongation at break is greater than 150%, and the deformation rate after long-time compression after high-temperature long-term compression is 1t; and after high-temperature aging, the adhesive is well adhered to an adhesive surface, is not adhered to a sealing surface, and has good detachability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of liquid silicone rubber, and specifically relates to an in-situ formed single-component addition type liquid silicone rubber and a preparation method thereof. Background Art

[0002] Liquid silicone rubber (LSR) is a polymer material composed of polymers, cross-linking agents and catalysts. Due to its unique structure, it combines the properties of inorganic and organic materials, and has basic properties such as small viscosity-temperature coefficient, high compressibility, and high low-temperature flexibility. It also has excellent properties such as high and low temperature resistance, electrical insulation, oxidation stability, weather resistance, flame retardancy, hydrophobicity, corrosion resistance, non-toxicity, odorlessness, and physiological inertness. It is widely used in aerospace, electronics, automotive industry, high-end construction and other industries, and has been tested in harsh real-world environments.

[0003] Condensation-type liquid silicone rubber mainly includes single-component and two-component products. The curing time of single-component condensation-type room temperature vulcanized liquid silicone rubber is long. Under typical environmental conditions (temperature 25°C, relative humidity 60%), the curing depth and strength gradually reach the design target value in about 3 weeks. Even with auxiliary conditions such as heating and humidification, its curing speed cannot be greatly improved. Relatively speaking, the two-component condensation-type room temperature vulcanized liquid silicone rubber can greatly improve the curing speed, but it still requires at least 24 hours of curing time to fully achieve the design performance. Condensation-type room temperature vulcanized liquid silicone rubber is not only unable to adapt to the assembly efficiency of the production line, but also has poor compression resilience and the release of low-molecular substances during the curing process, which will also limit its application as a sealing material for in-situ molding (in-situ molding refers to the process of first applying liquid sealant on the flange or other sealing surface, and then assembling after rapid curing to achieve single-sided bonding and double-sided compression sealing). Due to its unique cross-linking curing mechanism, addition-type liquid silicone rubber can achieve rapid curing by heating, good compression rebound, no low-molecular release, and is more environmentally friendly. Two-component addition-type silicone rubber needs to be measured by equipment according to the ratio of the two components, and then mixed evenly before use. During the metering and mixing process, there are phenomena of uneven metering and uneven mixing of the two components, which seriously affect the stability of product performance, thereby affecting the mechanical properties and compression permanent deformation properties. The one-component addition-type liquid silicone rubber is simpler and easier to use, and does not require complicated proportioning and mixing operations. It can not only save packaging materials and reduce resource waste, but also has the advantages of easy storage and transportation, and easy use. It can be seen that the one-component addition-type liquid silicone rubber is the best choice for preparing in-situ formed sealing materials.

[0004] Conventional one-component addition-type liquid silicone rubber is highly saturated due to the helical curling of the molecular chain segments and the polarity of the silicon-oxygen bond shielded by the non-polar side groups, showing low surface energy, poor wettability to various substrates, and lack of reactive groups. The molecular interaction between the substrate and the substrate is weak, and the bonding performance is poor. At present, the simplest and most effective method is to add a silane coupling agent to the system. Among the conventional silane coupling agents, amino coupling agents will cause the platinum catalyst to fail and cannot be used; epoxy coupling agents cannot participate in the cross-linking reaction, and the sealant is easy to precipitate after long-term compression after curing, which is not conducive to the long-term, safe and stable operation of the internal components of the seal; although acryloxy coupling agents can participate in the cross-linking reaction, they will affect the curing speed and mechanical properties; the more active methoxy or ethoxy groups in the silane coupling agent cause the cured rubber strip to continue to react with the substrate surface after long-term compression, resulting in adhesion, and non-destructive disassembly and repair cannot be achieved.

[0005] The existing in-situ formed single-component addition-type liquid silicone rubber generally has the problem of large dimensional change rate before and after high-temperature curing. Adding hydrophilic white carbon black or organic bentonite can improve it to a certain extent, but the extrusion is poor and the particles are obvious, which seriously affects the dispensing speed and the qualified rate of finished products; although the commercially available liquid thixotropic additives, hydrogenated castor oil and polyamide wax can effectively improve the thixotropic effect, they have poor compatibility with the single-component addition-type silicone rubber, large dimensional change rate before and after curing, and affect the curing speed, and cannot meet the requirements of good room temperature extrusion and low dimensional change rate before and after high-temperature curing. Therefore, it is very necessary to develop an in-situ formed single-component addition-type liquid silicone rubber, which not only has excellent bonding performance to metal substrates, small dimensional change rate before and after curing, but also has good bonding to the bonding surface after high-temperature aging, no bonding to the sealing surface, and good detachability.

[0006] At present, the key to the development of single-component addition-type liquid silicone rubber for in-situ forming and sealing is to solve the problems of bonding, dimensional retention before and after high-temperature curing, and removability after high-temperature aging. If good adhesion to the substrate is to be achieved, it is necessary to add an additional tackifier. Although the addition of conventional tackifiers can effectively improve the bonding effect, oil seepage and adhesion are prone to occur after high-temperature aging; if dimensional retention before and after high-temperature curing is to be achieved, it is necessary to add an additional thixotropic additive. Although it can effectively improve the thixotropic effect, it has poor extrudability or poor compatibility with the silicone matrix. One of the current methods to solve the above problems is to add low-activity thixotropic agents and tackifiers.

[0007] Chinese patent publication number CN110387128 A discloses a self-adhesive one-component addition-type silicone rubber and a preparation method thereof. Vinyl silicone oil and nano-silicon dioxide are kneaded to obtain a paste, which is then mixed with an appropriate proportion of cross-linking agent, tackifier, inhibitor and other additives for degassing. The preparation process is simple. The prepared silicone rubber product combines the advantages of condensation-type and addition-type silicone rubbers, has single-component packaging, no small molecule release during curing, no deep curing problem, fast curing by heating, easy to use, simple, efficient and other characteristics. More importantly, the components are combined in an appropriate proportion, so that it has good bonding properties to a variety of substrates, especially difficult-to-bond materials such as nickel, silver, gold, nylon 66, PVC, PE, etc., which greatly expands the application scope of the existing one-component addition-type silicone rubber. The disadvantages are that the tackifier is a polymerization product of borate and silane coupling agent, and has no active groups that can react with polymers or cross-linking agents, which will cause oil leakage in the cured rubber strip after long-term compression at high temperature. In addition, the tackifier contains a large number of hydrolyzable active groups such as methoxy and ethoxy, which will cause the cured rubber strip to continue to react with the surface of the substrate after long-term compression, resulting in adhesion, making it impossible to achieve non-destructive disassembly and repair.

[0008] Chinese patent publication number CN 115521625 A discloses a low-temperature bonding and boiling-resistant two-component addition-type silicone rubber and its preparation method. Component A consists of base rubber, vinyl-terminated silicone oil, reinforcing agent, and catalyst. Component B consists of base rubber, vinyl-terminated silicone oil, hydrogen-containing silicone oil, reinforcing agent, tackifier, water-resistant agent, and inhibitor. The base rubber consists of vinyl-terminated silicone oil, fumed silica, silane treatment agent, and water. By adding a new special tackifier and water-resistant agent, it can achieve rapid curing at a low temperature of 60°C and form a strong bond with the substrate. At the same time, the water-resistant agent containing long-chain phenyl silane has strong hydrophobicity and can significantly improve the boiling resistance. The bonding strength does not decrease significantly after boiling. Its disadvantage is that the two-component addition-type silicone rubber needs to be metered by equipment according to the ratio of the two components and then mixed evenly before use. During the metering and mixing process, there is a phenomenon of uneven metering and uneven mixing of the two components, which seriously affects the stability of the product performance, thereby affecting the mechanical properties and compression permanent deformation properties.

[0009] Chinese patent publication number CN110669344A discloses a one-component addition-type liquid silicone rubber and a preparation method thereof, comprising the following raw materials: 20 to 50 parts by weight of low-viscosity vinyl silicone oil, the viscosity of the low-viscosity vinyl silicone oil is 8000 to 12000 cs; high-viscosity vinyl silicone oil with a viscosity of 60000 to 80000 cs, the total amount of the high-viscosity vinyl silicone oil and the low-viscosity vinyl silicone oil is 70 parts by weight; 20 to 35 parts by weight of white carbon black; 5 to 8 parts by weight of hexamethyldisilazane; 1 to 5 parts by weight of high-vinyl silicone oil, the vinyl content of the high-vinyl silicone oil is 7% to 10%; 1.5 to 2 parts by weight of water; 2 to 4 parts by weight of hydrogen-containing silicone oil; 0.2 to 0.5 parts by weight of a platinum complex; and 0.02 to 0.08 parts by weight of 3-methyl-1-dodecyne-3-ol. The disadvantages are that the liquid silicone rubber without the addition of tackifier has low surface energy after curing, poor adhesion to the substrate, and a storage period of only 3 months at 25°C.

[0010] Chinese patent publication number CN102492391A discloses a one-component strong adhesive addition type silicone rubber encapsulation glue and its preparation method, which includes 80-120 parts of vinyl silicone oil, 5-20 parts of vinyl silicone resin, 10-30 parts of hydrogenated silicone oil, 1-3 parts of organopolysiloxane tackifier, 1-3 parts of white carbon black, 1-5 parts of titanium dioxide, 0.1-0.5 parts of inhibitor and 0.1-0.5 parts of platinum catalyst by weight. The preparation method is to firstly stir and mix vinyl silicone oil, vinyl silicone resin, hydrogenated silicone oil, organopolysiloxane tackifier, white carbon black and titanium dioxide at high speed; then add the inhibitor and stir and mix at high speed; finally add the platinum catalyst and stir and mix at high speed, and discharge the material. The one-component addition type silicone rubber encapsulation glue prepared by this method has a bonding strength of more than 1.86MPa with the substrate (copper) after vulcanization. The disadvantage is that although the organopolysiloxane tackifier can participate in the hydrosilylation crosslinking reaction and can avoid the problem of long-term compression seepage to a certain extent, the sizing material has poor thixotropy after being added and has a large dimensional change rate before and after high-temperature curing. Summary of the invention

[0011] In order to overcome the deficiencies and disadvantages of the prior art, the primary purpose of the present invention is to provide a one-component addition-type liquid silicone rubber for in-situ molded sealing, which uses a tackifier and a thixotropic agent and has a special structure.

[0012] The second object of the present invention is to provide a method for preparing the one-component addition-type liquid silicone rubber for in-situ molded sealing.

[0013] The primary purpose of the present invention is achieved through the following technical solutions:

[0014] A one-component, in-situ forming liquid silicone rubber, measured by weight, is made of raw materials including the following materials:

[0015]

[0016] Wherein the base material is made of raw materials including the following materials:

[0017] 65 parts of vinyl silicone oil,

[0018] 15-50 parts of fumed silica,

[0019] 10 to 30 parts of silicone resin.

[0020] Preferably, the hydrogen-containing silicone oil is a double-terminal methyl-side hydrogen-containing silicone oil with a hydrogen content of 0.36% to 1.6%. It is purchased and selected for use according to the demand for hydrogen content. The structural formula is as follows:

[0021] g is a natural number between 15 and 100, and h is a natural number between 1 and 100; g is a natural number between 15 and 100 means that g can be any one of 15, 20, 30, 40, 50, 60, 70, 80, 90 or 100, or any other natural number between 15 and 100; similarly, h is a natural number between 1 and 100 means that h can be any one of 5, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, or any other natural number between 1 and 100;

[0022] Preferably, the inhibitor is at least one of 3-methyl-1-dodecene-3-ol, 3,7,11-trimethyldodecene-3-ol, 3-methyl-1-butyn-3-ol, 1-ethynyl-1-cyclohexanol, and 3-phenyl-1-butyn-3-ol;

[0023] Preferably, the catalyst is a platinum-alkyne-based complex, i.e., at least one of bis(1-ethynyl-1-cyclohexanol)bis(triphenylphosphine)platinum complex, bis(phenylacetylene)bis(triphenylphosphine)platinum complex, bis(alkyneoxysiloxane)bis(triphenylphosphine)platinum complex, and bis(3-methyl-1-butyn-3-ol)bis(triphenylphosphine)platinum complex, wherein the platinum content is 1000 to 3000 ppm.

[0024] Preferably, the vinyl silicone oil has a viscosity of 5000 to 20000 mPa.s at a temperature of 25° C. and a vinyl content of 0.05% to 0.2%. The vinyl silicone oil is purchased and selected for use according to the demand for vinyl content. The structural formula is as follows:

[0025] F is a natural number between 1 and 100; F is a natural number between 1 and 100 means that F can be any number such as 5, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, or any other natural number between 1 and 100;

[0026] Preferably, the specific surface area of ​​the fumed silica is 200 to 400 m 2 / g, fumed silica includes hydrophilic fumed silica and hydrophobic fumed silica; hydrophobic fumed silica (such as fumed silica treated with hexamethyldisilazane) is preferred, because excessive addition of hydrophilic fumed silica will lead to a higher consistency of liquid silicone rubber, which is not conducive to use, while hydrophobic fumed silica can not only be used in a higher addition amount, but also will not cause the rubber to be structured, which is conducive to long-term storage stability. However, the addition amount of hydrophobic silica cannot be too much, so it is used with silicone resin to meet better extrusion performance and mechanical properties.

[0027] Preferably, the silicone resin is phenyl vinyl MDQ silicone resin, with a viscosity of 500-1000 mPa.s at 25°C and a vinyl content of 0.4%-1%. It is purchased and selected for use according to the demand for vinyl content. The general structural formula is: (Ph 2 SiO)a(ViMe 2 SiO 0.5 )b(Me 3 SiO 0.5 )c(SiO 2 )d, wherein Ph is phenyl, Me is methyl, Vi represents vinyl; the value range of a is 0.1 to 1; the value range of b+c is 0 to 0.1, and b>0; the value range of d is 0 to 0.8, and d>0; the value range of a / d is 1.6 to 2.5; the value range of (b+c) / d is 1.6 to 2.5. Since the cohesive energy density of silicone polymers is small, they need to be reinforced by reinforcing materials. The most common and most used reinforcing filler is fumed or precipitated silica, but it also has a very obvious thickening effect on silicone rubber, which will increase the viscosity of the rubber and affect the actual application range of silicone rubber. Therefore, phenyl vinyl MDQ silicone resin containing Q segments with a structure similar to fumed silica is used to reinforce it; phenyl vinyl MDQ silicone resin and silicone polymer containing silicon-hydrogen bonds (i.e., hydrogen-containing silicone oil) undergo a hydrogen silanization addition reaction under the action of a catalyst to cross-link and vulcanize, which can significantly improve the cohesive energy density and heat resistance of the silicone polymer, so that the cured silicone rubber has better mechanical properties and compression rebound properties.

[0028] Thickener and preparation method thereof:

[0029] The method for preparing a tackifier used in a one-component addition-type liquid silicone rubber formed in situ comprises the following steps:

[0030] (1) Tetramethylcyclotetrasiloxane (D 4 H) and the catalyst are stirred evenly, 2-epoxy-4-vinylcyclohexane (VCMX) and bisphenol A bisallyl ether are added, the temperature is raised to 50°C to 100°C and the reaction is carried out for 2h to 5h;

[0031] (2) After cooling to room temperature, add activated carbon for adsorption for 8 h to 24 h, filter, and perform vacuum distillation to obtain a thickener.

[0032] The tackifier used in the in-situ one-component addition type liquid silicone rubber has the following structure:

[0033] Call it product A.

[0034] Optionally, in the preparation method of the tackifier, D 4 The molar ratio of H, catalyst, 2-epoxy-4-vinylcyclohexane (VCMX), and bisphenol A bisallyl ether is (100-200): 1: (100-200):

[0035] (50~100), the preferred molar ratio is (120~160):1:(120~160):(60~80).

[0036] Preferably, in the method for preparing the tackifier, the catalyst in step (1) is at least one of chloroplatinic acid and Karstedt platinum catalyst.

[0037] Thixotropic agent and its preparation method:

[0038] The method for preparing a thixotropic agent used in a one-component addition-type liquid silicone rubber formed in situ comprises the following steps:

[0039] (1) Stir hydrogenated polydimethylsiloxane and catalyst evenly, add additive 1, heat to 50°C to 100°C and react for 2h to 5h;

[0040] (2) After cooling to room temperature, add activated carbon for adsorption for 8 h to 24 h, filter, and distill under reduced pressure to obtain a thixotropic agent.

[0041] In the preparation method of the thixotropic agent, the hydrogen-containing polydimethylsiloxane in step (1) is at least one of single-end hydrogen polydimethylsiloxane, double-end hydrogen polydimethylsiloxane, side hydrogen-containing polydimethylsiloxane or end-side hydrogen polydimethylsiloxane.

[0042] In the preparation method of the thixotropic agent, the auxiliary agent 1 in step (1) is at least one of 1,2-epoxy-4-vinylcyclohexane (VCMX), allyl glycidyl ether (AGE), and dodecene.

[0043] Preferably, when the auxiliary agent 1 is 2-epoxy-4-vinylcyclohexane (VCMX), and the hydrogen-containing polydimethylsiloxane is a pendant hydrogen-containing polydimethylsiloxane, the prepared thixotropic agent has the following structure:

[0044] Call it product B, p is a natural number between 1 and 100, n is a natural number between 1 and 100, and m is a natural number between 1 and 100. p, m, and n can be any natural number such as 5, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, or other natural numbers between 1 and 100;

[0045] Optionally, in the preparation method of the thixotropic agent, the molar ratio of hydrogen-containing polydimethylsiloxane, the catalyst, and the auxiliary agent 1 is (100-150):1:(20-50), and the preferred molar ratio is (110-120):1:(30-40).

[0046] Preferably, in the method for preparing a thixotropic agent, the catalyst in step (1) is at least one of chloroplatinic acid and Karstedt platinum catalyst.

[0047] The small molecule thixotropic agent has a siloxane main chain and has good compatibility with liquid silicone rubber. It is beneficial for the epoxy groups on the thixotropic agent to form hydrogen bonds with the hydroxyl groups on the hydrophobic fumed silica (such as hexamethyldisilazane-treated silica) of the base rubber reinforcing filler, thereby better exerting the thixotropic effect.

[0048] In the present invention, room temperature generally refers to a temperature within the range of 20 to 35° C., which varies naturally with the environment.

[0049] The second object of the present invention is achieved by the following technical solutions:

[0050] A method for preparing an in-situ formed single-component addition-type liquid silicone rubber, the method comprising the following steps:

[0051] (1) Preparation of base material:

[0052] 65 parts by mass of vinyl silicone oil, 15 to 50 parts by mass of fumed silica and 10 to 30 parts by mass of silicone resin are stirred in a vacuum kneader for 30 to 120 minutes, heated to 120° C. to 200° C., and then de-blended at a vacuum degree of -0.08 to -0.1 MPa for 60 to 180 minutes, diluted, cooled and ground to obtain a base material;

[0053] (2) Preparation of in-situ single-component addition-type liquid silicone rubber:

[0054] 100 parts by mass of base material and 2-8 parts by mass of hydrogenated silicone oil are added into a planetary mixer with a cooling and high-speed dispersing device, and stirred for 15-20 minutes at a high-speed dispersing speed of 300-600 r / min, a low-speed stirring speed of 30-60 r / min, and a vacuum degree of -0.08 to -0.1 MPa. 1-5 parts by mass of tackifier and 1-5 parts by mass of thixotropic agent are added, and stirred for 10-30 minutes at a high-speed dispersing speed of 500-1000 r / min and a low-speed stirring speed of 40-80 r / min. 0.05-1 parts by mass of inhibitor and 0.1-1 parts by mass of catalyst are added, and stirred for 5-15 minutes at a high-speed dispersing speed of 300-600 r / min, a low-speed stirring speed of 30-60 r / min, and a vacuum degree of -0.08 to -0.1 MPa. The material is discharged, sealed, and stored to obtain a single-component addition-type liquid silicone rubber for in-situ molding sealing.

[0055] Working principle of the present invention:

[0056] The one-component addition-type liquid silicone rubber for in-situ forming and sealing of the present invention utilizes phenyl vinyl MDQ silicone resin and organic silicon polymer containing silicon hydrogen bond to undergo hydrogen siloxane addition reaction under the action of catalyst to crosslink and vulcanize, which can significantly improve the cohesive energy density and heat resistance of organic silicon polymer, so that the cured silicone rubber has good mechanical properties and compression resilience, so the two are selected for use. A hydrogen-containing cyclic siloxane tackifier with epoxy and benzene ring groups is designed and synthesized, which not only has good compatibility with the organic silicon matrix, but also Si-H can participate in the crosslinking reaction to introduce epoxy and benzene ring groups into the main chain. The epoxy group has low activity at room temperature, and can react with the surface active group of the substrate to form a strong bonding effect when heated at high temperature. After the one-component addition-type liquid silicone rubber with the tackifier is cured at high temperature, due to the spiral curling of the molecular chain segment and the polarity of the epoxy group and the silicon oxygen bond shielded by the non-polar benzene ring macromolecule and the side group, the whole molecule is highly saturated, showing a low surface energy, and the molecular interaction force with the substrate is weak, thereby avoiding oil seepage and adhesion during long-term compression. The mechanical properties are improved by adding hydrophobic fumed silica, but excessive addition will lead to obvious thickening of silicone rubber and increased viscosity of the rubber, which will affect the actual application range of silicone rubber. The present invention designs and synthesizes a hydrogen-containing polydimethylsiloxane (thixotropic agent) with epoxy groups in the side chain, which relies on the relatively large number of oxygen atoms on the epoxy groups to produce stable hydrogen bonds with the hydrophobic fumed silica in the system that plays a reinforcing role, thereby producing a thixotropic effect without affecting the extrudability. At the same time, a siloxane segment is introduced into the thixotropic agent structure to increase the compatibility of the thixotropic agent with the silicone matrix to better exert the thixotropic effect, and effectively avoid the risk of incompatible seepage between the thixotropic agent and the rubber system, thereby solving the problems of large dimensional changes before and after curing and poor extrudability of the single-component addition-type sealant.

[0057] The planetary mixer contains a high-speed dispersion disk, i.e. high-speed stirring, and shear stirring, i.e. low-speed stirring. High-speed stirring and dispersion are performed first, and then low-speed stirring is performed to obtain a better dispersion effect.

[0058] In the present invention, the term "deoxidation" refers to the removal of small molecules.

[0059] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0060] (1) The one-component addition-type liquid silicone rubber for in-situ form-sealing prepared by the present invention has good mechanical properties (tensile strength>5Mpa, elongation at break>150%), good adhesion to metal substrates (AL-AL shear strength>2Mpa) and excellent compression resilience (compression permanent deformation rate <30% after compression of 25% and aging at 150°C for 1000h).

[0061] (2) By designing and synthesizing a multifunctional hydrogen-containing cyclic tackifier, the tackifier reacts with the main resin, epoxy siloxane and benzene rings are introduced into the sealant, the surface polarity of the sealant is changed, the wettability to the substrate is improved, and thus the bonding performance is improved. At the same time, the tackifier itself does not carry alkoxy groups, so the hydrolyzable alkoxy components inside the colloid can be reduced to prevent subsequent adhesion. The test results show that the anti-adhesion level is high, because the alkoxy groups will continue to react in the later stage of glue curing, thereby causing glue adhesion. The one-component addition-type liquid silicone rubber for in-situ molding sealing prepared with this tackifier solves the technical problems of poor adhesion to the substrate and compression sealing adhesion of conventional coupling agents and commercially available tackifiers added to one-component addition-type liquid silicone rubber.

[0062] (3) By designing and synthesizing a thixotropic agent grafted with epoxy groups, it not only has good compatibility with the silicone rubber system, but also can participate in the cross-linking reaction to prevent exudation. The one-component addition-type liquid silicone rubber for in-situ molding and sealing prepared with this thixotropic agent not only has good extrusion properties at room temperature, but also has excellent thixotropy at high temperatures. The test results show that the dimensional change before and after high-temperature curing is small, which solves the contradiction between the poor extrusion properties of addition-type silicone rubber at room temperature and the dimensional change during high-temperature curing. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] Figure 1 It is the reaction equation for preparing the thickener.

[0064] Figure 2 It is the reaction equation for preparing thixotropic agent.

[0065] Figure 3 It is a standard jig for gluing.

[0066] Figure 4 This is a schematic diagram of the effect of thixotropic agent and white carbon black. DETAILED DESCRIPTION

[0067] The present invention is specifically described below through examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art in this field can make some non-essential improvements and adjustments based on the contents of the present invention.

[0068] The preparation method of the tackifier described in Example 1 is as follows:

[0069] In a three-necked flask equipped with a thermometer, condenser, and mechanical stirring device, add 0.3 mol of tetramethylcyclotetrasiloxane (D 4 H) and 0.002 mol Custer platinum catalyst (5000 ppm) were stirred for 15 min, 0.3 mol 2-epoxy-4-vinylcyclohexane (VCMX) and 0.14 mol bisphenol A bisallyl ether were added, and the temperature was raised to 80°C for reaction for 3 h; after cooling to room temperature, activated carbon was added for adsorption for 24 h, filtered, and distilled under reduced pressure to obtain product A. The reaction equation is as follows Figure 1 shown.

[0070] The preparation method of the thixotropic agent described in Example 1 is as follows:

[0071] In a three-necked flask equipped with a thermometer, a condenser and a mechanical stirring device, 0.115 mol of side-hydrogenated polydimethylsiloxane with a hydrogen content of 1.2% and 0.001 mol of Custer platinum catalyst (5000 ppm) were added and stirred for 15 minutes. 0.035 mol of 1,2-epoxy-4-vinylcyclohexane (VCMX) was added and the temperature was raised to 90°C for reaction for 2 hours. After cooling to room temperature, activated carbon was added for adsorption for 24 hours, filtered and distilled under reduced pressure to obtain product B.

[0072] The reaction equation is Figure 2 As shown, Figure 2 The t and m in the figure are determined by the hydrogen content of the hydrogen-containing silicone oil.

[0073] The preparation method of the thixotropic agent described in Example 2 is as follows:

[0074] In a three-necked flask equipped with a thermometer, a condenser and a mechanical stirring device, add 0.110 mol of side-hydrogenated polydimethylsiloxane with a hydrogen content of 1.2% and 0.001 mol of Custer platinum catalyst (5000 ppm) and stir for 15 min. Add 0.038 mol of allyl glycidyl ether (AGE) and heat to 90°C to react for 2 h. After cooling to room temperature, add activated carbon for adsorption for 24 h, filter and distill under reduced pressure to obtain product B1.

[0075] The preparation method of the thixotropic agent described in Example 3 is as follows:

[0076] In a three-necked flask equipped with a thermometer, a condenser and a mechanical stirring device, add 0.120 mol of side-hydrogenated polydimethylsiloxane with a hydrogen content of 1.2% and 0.001 mol of Custer platinum catalyst (5000 ppm) and stir for 15 min. Add 0.030 mol of dodecene and heat to 90°C to react for 2 h. After cooling to room temperature, add activated carbon for adsorption for 24 h, filter and distill under reduced pressure to obtain product B2.

[0077] Embodiment 1:

[0078] 65 parts by mass of vinyl silicone oil with a viscosity of 10000 mPa.s and a specific surface area of ​​300 m 2 / g of hydrophobic fumed silica 15 parts by mass and phenyl vinyl MDQ silicone resin with a vinyl content of 0.58% are added into a vacuum kneader and stirred for 30 minutes, then heated to 120°C and stirred for 60 minutes, and then de-blended at 160°C and a vacuum degree of -0.08Mpa for 120 minutes, then diluted, cooled and ground to obtain a base material.

[0079] 3 parts by mass of side hydrogen-containing silicone oil with a hydrogen content of 0.75% and 100 parts by mass of base material were added into a planetary mixer, mixed and stirred for 15 minutes at a high-speed dispersion of 500 r / min, a low-speed stirring of 50 r / min, and a vacuum degree of -0.08 MPa (the stirring conditions of the following embodiments and comparative examples are the same as those of Example 1), and then 1 part by mass of product A and product B were added, and the mixture was stirred and mixed for 20 minutes at a high-speed dispersion of 750 r / min and a low-speed stirring of 60 r / min. Then, 0.15 parts by mass of bis(1-ethynyl-1-cyclohexanol)bis(triphenylphosphine)platinum complex (platinum content of 3000 ppm) and 0.05 parts by mass of 1-ethynyl-1-cyclohexanol were added, and the mixture was stirred for 15 minutes at a high-speed dispersion of 400 r / min and a low-speed stirring of 45 r / min while maintaining a vacuum degree of -0.099 MPa. After the mixture was discharged and sealed for storage, a single-component addition-type liquid silicone rubber for in-situ molding sealing was obtained, which was marked as finished product C1.

[0080] Embodiment 2:

[0081] The preparation process is similar to that of Example 1, except that an equal amount of product B in Example 1 is replaced by product B1, which is marked as finished product C2.

[0082] Embodiment 3:

[0083] The preparation process is similar to that of Example 1, except that an equal amount of product B in Example 1 is replaced by product B2, which is marked as finished product C3.

[0084] Embodiment 4:

[0085] The preparation process is similar to that of Example 1, except that the silicone resin in Example 1 is replaced with an equal mass of phenyl vinyl MDQ silicone resin with a vinyl content of 0.45%, and 2.6 parts by mass of side hydrogenated silicone oil with a hydrogen content of 0.75%, which is marked as finished product C4.

[0086] Embodiment 5:

[0087] The preparation process is similar to that of Example 1, except that the silicone resin in Example 1 is replaced with an equal mass of phenyl vinyl MDQ silicone resin with a vinyl content of 0.66%, and 3.5 parts by mass of side hydrogenated silicone oil with a hydrogen content of 0.75%, which is marked as finished product C5.

[0088] Embodiment 6:

[0089] The preparation process is similar to that of Example 1, except that 3 parts by mass of the side hydrogen-containing silicone oil with a hydrogen content of 0.75% in Example 1 is replaced by 2 parts by mass of the side hydrogen-containing silicone oil with a hydrogen content of 1.2%, which is marked as finished product C6.

[0090] Comparative Example 1:

[0091] 65 parts by mass of vinyl silicone oil with a viscosity of 10000 mPa.s and a specific surface area of ​​300 m 2 / g of hydrophobic fumed silica 15 parts by mass and phenyl vinyl MDQ silicone resin with a vinyl content of 0.58% are added into a vacuum kneader and stirred for 30 minutes, then heated to 120°C and stirred for 60 minutes, and then vacuumed at 160°C and a vacuum degree of -0.08Mpa for 120 minutes, then diluted, cooled and ground to obtain a base material.

[0092] 3 parts by mass of side hydrogen-containing silicone oil with a hydrogen content of 0.75% and 100 parts by mass of base material were added into a three-dimensional high-speed disperser, and mixed and stirred for 15 minutes at a high-speed dispersion of 500 r / min, a low-speed stirring of 50 r / min, and a vacuum degree of -0.08 MPa (the stirring conditions of the following embodiments and comparative examples are the same as those of Example 1), 0.15 parts by mass of bis(1-ethynyl-1-cyclohexanol)bis(triphenylphosphine)platinum complex (platinum content 3000 ppm) and 0.05 parts by mass of 1-ethynyl-1-cyclohexanol were added, and the mixture was stirred for 15 minutes at a high-speed dispersion of 400 r / min and a low-speed stirring of 45 r / min while maintaining a vacuum degree of -0.099 MPa. After the mixture was discharged and sealed for storage, a single-component addition-type liquid silicone rubber was obtained, which was marked as finished product C7.

[0093] Comparative Example 2:

[0094] The preparation process is similar to that of Comparative Example 1, except that the mass of phenyl vinyl MDQ is replaced by vinyl silicone oil with a viscosity of 10000 mPa.s at a temperature of 25°C and 2 parts by mass of side hydrogenated silicone oil with a hydrogen content of 0.75%, marked as finished product C8.

[0095] Comparative Example 3:

[0096] The preparation process is similar to that of Example 1, except that product A is not added and is marked as finished product C9.

[0097] Comparative Example 4:

[0098] The preparation process is similar to that of Example 1, except that product A is replaced by a commercially available tackifier, which is labeled as finished product C10.

[0099] Performance Testing

[0100] a. Adhesion and mechanical properties test

[0101] The finished products C1-C9 were prepared according to GB / T 7124-2008 and GB / T 528-2009 standards, placed in a 150°C forced air drying oven for curing for 30 minutes, and then taken out and placed at room temperature for 2 hours before shear strength (test substrate is 3003 aluminum), tensile strength and elongation at break tests. The test results are shown in Table 1:

[0102] Table 1 Comparison of mechanical properties of examples and comparative examples

[0103] Finished product number Shear strength, Mpa Tensile strength, MPa Elongation at break, % C1 3.6 5.2 300 C2 3.52 5.3 290 C3 3.5 5.1 290 C4 3.3 4.6 320 C5 3.5 5.8 260 C6 3.8 5.6 230 C7 0.6 4.7 320 C8 0.58 4.2 360 C9 1.2 4.9 300 C10 2.0 4.8 270

[0104] Compared with Example 1, Example 2 and Example 3 used different thixotropic agents, and the obtained liquid silicone rubbers all had higher shear strength, tensile strength and elongation at break, indicating that the liquid silicone rubbers of Examples 1 to 3 had better bonding properties.

[0105] Compared with Example 1, the vinyl content of phenyl vinyl MDQ silicone resin in Example 4 is reduced, and the amount of hydrogen-containing silicone oil is reduced; compared with Example 1, the vinyl content of phenyl vinyl MDQ silicone resin in Example 5 is increased, and the amount of hydrogen-containing silicone oil is increased; the mechanical properties of the three are not much different, indicating that the vinyl content of phenyl vinyl MDQ silicone resin and the amount of hydrogen-containing silicone oil can be adjusted within a certain range. Compared with C5, the shear strength and tensile strength of C6 are improved, but the elongation at break is reduced.

[0106] Compared with Example 1, the hydrogen content of the hydrogen-containing silicone oil in Example 6 is increased, but the dosage is reduced, and a glue with high shear strength and tensile strength can still be obtained, but the elongation at break is reduced to a certain extent. This shows that the hydrogen content and dosage of the hydrogen-containing silicone oil can be adjusted within a certain range of the total hydrogen content.

[0107] Compared with Example 1, Comparative Examples 1 and 2 do not use a tackifier and a thixotropic agent, so the shear strength is very poor, indicating poor bonding performance.

[0108] Compared with Example 1, Comparative Example 3 did not use a tackifier, so the shear strength was very poor, indicating poor bonding performance. Compared with Comparative Example 1, Comparative Example 3 used a thixotropic agent, so the bonding performance was improved.

[0109] b. Dimensional change rate and high temperature anti-adhesion test

[0110] The finished products C1-C9 were coated with test samples using a coating device. Figure 3 On the standard fixture shown, the strip has a width of (3±0.5) mm and a height of (2.0±0.2) mm. After being cured in a 150°C air drying oven for 30 minutes, the dimensional change rate is tested. Then, the fixture is covered with a top cover and the screws are tightened with a torque screwdriver. The torque requirement is between 1.5 and 5.0 NM. After being aged in a 110°C air drying oven for 1000 hours, the anti-adhesion performance is tested according to GB / T 23982-2009. The test results are shown in Table 2:

[0111] Table 2 Comparison of dimensional change rate and high temperature anti-adhesion test between the embodiment and the comparative example

[0112]

[0113]

[0114] As can be seen from Tables 1 and 2, after adding product A, the shear strength of the liquid silicone rubber is greater than 3Mpa, and the anti-adhesion grade can reach A0, indicating that the liquid silicone rubber has good bonding performance and good detachability. This is mainly because Si-H in product A can participate in the cross-linking reaction to introduce epoxy and benzene ring groups into the main chain. The epoxy group has low activity at room temperature and can react with the surface active groups of the substrate to form a strong bonding effect when heated at high temperature. After high-temperature curing, due to the spiral curling of the molecular chain segments and the non-polar benzene ring macromolecules and side groups shielding the polarity of the epoxy group and the silicon oxygen bond, the entire molecule is highly saturated, showing a low surface energy, and the molecular interaction force with the substrate is Weak, thus avoiding oil seepage and adhesion during long-term compression, thereby achieving excellent anti-adhesion effect; after high-temperature curing with the addition of thixotropic agents B and B1, the dimensional change rate is within 5%, and after high-temperature curing with the addition of B2, the dimensional change rate is within 20%. Without the addition of a thixotropic agent, the dimensional change rate after high-temperature curing is relatively large, reaching more than 20%. This is mainly because more epoxy groups are introduced into the structures of B and B1. Due to the strong electronegativity of oxygen atoms, more oxygen atoms on the epoxy groups produce stable hydrogen bonds with the reinforcing silica in the system to produce a thixotropic effect. At the same time, siloxane segments are introduced into the structure to increase the compatibility of the thixotropic agent with the silicone oil base polymer, thereby better exerting the thixotropic effect. The thixotropic effect produced by the thixotropic agent is as follows: Figure 4 shown.

[0115] c. Compression permanent deformation performance test

[0116] The finished products C1-C9 were extruded into a polytetrafluoroethylene mold with a cavity thickness of (2.1±0.1) mm, placed in a 150°C blast drying oven for curing for 30 min, and placed at room temperature for 2 h. The samples were removed and cut into test pieces with a diameter of (13±0.5) mm and a thickness of (2.1±0.1) mm on a cutting machine. Three pieces were stacked to form a type B test piece specified in GB / T7759.1-2015. The compression permanent deformation rate test was carried out in accordance with GB / T 7759.1-2015 standard. The test conditions were: aging temperature 150°C, compression rate 25%, aging time 1000 h. The test results are shown in Table 3:

[0117] Table 3 Comparison of compression set rate test between examples and comparative examples

[0118] Finished product number Compression set C1 23% C2 26% C3 28% C4 29% C5 23% C6 22% C7 27% C8 32% C9 25% C10 30%

[0119] Compared with Comparative Example 1, Comparative Example 2 does not use phenyl vinyl MDQ silicone resin. As can be seen from Table 3, the compression set rate of Comparative Example 2 is higher than that of Comparative Example 1. Adding phenyl vinyl MDQ silicone resin can effectively improve the mechanical properties and compression set rate of liquid silicone rubber, and the compression set rate remains within 30% after aging at 150°C for 1000h. This is mainly because phenyl vinyl MDQ silicone resin can significantly improve the cohesive energy density and heat resistance of organic silicone polymers, and due to the steric hindrance rigidity effect of the benzene ring and the dense cross-linking points of the polyvinyl functional groups of the silicone resin, the cured silicone rubber has good mechanical properties and compression rebound properties, thereby giving the liquid silicone rubber excellent compression set performance.

[0120] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A one-component addition-type liquid silicone rubber that is formed in situ. It is characterized in that Made of the following materials in parts by mass: Wherein the base material is made of raw materials including the following materials: 65 parts of vinyl silicone oil, 15-50 parts of hydrophobic fumed silica, 10 to 30 parts of silicone resin.

2. The in-situ formed one-component addition type liquid silicone rubber according to claim 1, It is characterized in that The hydrogen-containing silicone oil is a double-terminal methyl-side hydrogen-containing silicone oil with a hydrogen content of 0.36% to 1.6%. The structural formula is as follows: g is a natural number between 15 and 100, and h is a natural number between 1 and 100.

3. The in-situ formed one-component addition type liquid silicone rubber according to claim 1, It is characterized in that The tackifier has the following structure:

4. The in-situ formed one-component addition type liquid silicone rubber according to claim 1, It is characterized in that The preparation method of the tackifier comprises the following steps: (1) Tetramethylcyclotetrasiloxane and a catalyst are stirred uniformly, 2-epoxy-4-vinylcyclohexane and bisphenol A bisallyl ether are added, the temperature is raised to 50° C. to 100° C., and the reaction is carried out for 2 h to 5 h; the molar ratio of tetramethylcyclotetrasiloxane, catalyst, 2-epoxy-4-vinylcyclohexane, and bisphenol A bisallyl ether is (100 to 200):1:(100 to 200):(50 to 100); the catalyst is chloroplatinic acid or Karstedt platinum catalyst; (2) After cooling to room temperature, add activated carbon for adsorption for 8 h to 24 h, filter, and perform vacuum distillation to obtain a thickener.

5. The method for preparing a one-component addition-type liquid silicone rubber formed in situ according to claim 1, It is characterized in that The thixotropic agent has the following structure: Wherein p is a natural number between 1 and 100, n is a natural number between 1 and 100, and m is a natural number between 1 and 100.

6. The method for preparing the in-situ formed one-component addition type liquid silicone rubber according to claim 1, It is characterized in that The preparation method of the thixotropic agent comprises the following steps: (1) Stirring hydrogenated polydimethylsiloxane and a catalyst uniformly, adding an auxiliary agent 1 and heating to 50°C to 100°C for reaction for 2h to 5h; the auxiliary agent 1 is at least one of 1,2-epoxy-4-vinylcyclohexane, allyl glycidyl ether, and dodecene; the molar ratio of hydrogenated polydimethylsiloxane, the catalyst, and the auxiliary agent 1 is (100 to 150):1:(20 to 50); the catalyst is chloroplatinic acid or a Karstedt platinum catalyst; (2) After cooling to room temperature, add activated carbon for adsorption for 8 h to 24 h, filter, and distill under reduced pressure to obtain a thixotropic agent.

7. The method for preparing the in-situ formed one-component addition type liquid silicone rubber according to claim 1, It is characterized in that The inhibitor is at least one of 3-methyl-1-dodecene-3-ol, 3,7,11-trimethyldodecene-3-ol, 3-methyl-1-butyn-3-ol, 1-ethynyl-1-cyclohexanol, and 3-phenyl-1-butyn-3-ol; the catalyst is at least one of bis(1-ethynyl-1-cyclohexanol)bis(triphenylphosphine)platinum complex, bis(phenylacetylene)bis(triphenylphosphine)platinum complex, bis(alkyneoxysiloxane)bis(triphenylphosphine)platinum complex, and bis(3-methyl-1-butyn-3-ol)bis(triphenylphosphine)platinum complex, wherein the platinum content is 1000 to 3000 ppm.

8. The method for preparing the in-situ formed one-component addition type liquid silicone rubber according to claim 1, It is characterized in that The specific surface area of ​​the hydrophobic fumed silica is 200 to 400 m 2 / g.

9. A method for preparing a one-component addition-type liquid silicone rubber for in-situ molding according to claim 1, It is characterized in that The vinyl silicone oil has a viscosity of 5000-20000 mPa.s at a temperature of 25°C, a vinyl content of 0.05%-0.2%, and a structural formula as follows: F is a natural number between 1 and 100; the silicone resin is phenyl vinyl MDQ silicone resin, and the vinyl content is 0.4% to 1%.

10. A method for preparing an in-situ formed one-component addition type liquid silicone rubber, It is characterized in that The following steps are involved: (1) Preparation of base material: 65 parts by mass of vinyl silicone oil, 15 to 50 parts by mass of fumed silica and 10 to 30 parts by mass of silicone resin are stirred in a vacuum kneader for 60 to 120 minutes, heated to 120° C. to 200° C., and then de-blended at a vacuum degree of -0.08 to -0.1 MPa for 60 to 180 minutes, diluted, cooled and ground to obtain a base material; (2) Preparation of in-situ single-component addition-type liquid silicone rubber: 100 parts by weight of base material and 2-8 parts by weight of hydrogenated silicone oil are added into a planetary mixer with a cooling and high-speed dispersing device, and stirred for 15-20 minutes at a high-speed dispersing speed of 300-600 r / min, a low-speed stirring speed of 30-60 r / min, and a vacuum degree of -0.08--0.1 MPa. 1-5 parts by weight of a tackifier and 1-5 parts by weight of a thixotropic agent are added, and stirred for 10-30 minutes at a high-speed dispersing speed of 500-1000 r / min and a low-speed stirring speed of 40-80 r / min. 0.05-1 parts by weight of an inhibitor and 0.1-1 parts by weight of a catalyst are added, and stirred for 5-15 minutes at a high-speed dispersing speed of 300-600 r / min, a low-speed stirring speed of 30-60 r / min, and a vacuum degree of -0.08--0.1 MPa. The material is discharged, sealed, and stored to obtain an in-situ formed single-component addition-type liquid silicone rubber.

Citation Information

Patent Citations

  • Organic silicone thixotropic agent and thixotropy addition type liquid silicone rubber

    CN103937257A

  • Tackifier, secondary vulcanization-free self-adhesive addition type liquid silicone rubber and preparation method of silicone rubber

    CN115960358A

  • Addition-type silicone rubber having high adhesive strength and preparation method therefor

    WO2022140877A1

Cited By

  • Platinum complex as well as preparation method and application thereof

    CN120058807A

  • Organosilicon fiber and preparation method thereof

    CN120649193A

  • Silicone fibers and methods for making the same

    CN120649193B

  • Single-component organic silicon hot laminating adhesive capable of being cured in segmented manner as well as preparation method and application of single-component organic silicon hot laminating adhesive

    CN121759152A

  • Low-viscosity high-temperature collapse-resistant high-strength thermocuring silicone rubber as well as preparation method and application thereof