PEM membrane electrode assembly for hydrogen production through water electrolysis and preparation method of PEM membrane electrode assembly
By using multi-layer structural membrane electrode assembly and gradient perfluorosulfonic acid ionomer in PEM electrolytic hydrogen production technology, the problems of poor swelling and binding force of membrane electrodes are solved, the electrochemical performance and life are improved, and the further development is achieved. High current density and lower catalyst loading.
Patent Information
- Application Number
- CN202411249264.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-26
AI Technical Summary
In the existing PEM electrolytic hydrogen production technology, when the membrane electrode is prepared by the CCM method, the proton exchange membrane is prone to swelling and deformation, and the bonding force between the catalyst layer and the gas diffusion layer is poor, resulting in attenuation of electrochemical performance and reduced service life.
The membrane electrode assembly design adopts a multi-layer structure, including the gradient distribution of the cathode and anode catalyst layers, the gradient of the perfluorosulfonic acid ionomer content, and the catalyst layer and the proton exchange membrane are closely combined through the transfer method to reduce the catalyst layer and the Contact resistance of the gas diffusion layer.
It improves the electrochemical performance and stability of the membrane electrode, reduces the catalyst load, improves the current density and electrochemical performance, and extends the service life.
Smart Images

Figure CN119020800A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a membrane electrode assembly for PEM water electrolysis to produce hydrogen and a preparation method thereof. Background Art
[0002] Hydrogen energy has received great attention from industry, academia and research at home and abroad due to its high calorific value, sustainability, abundant reserves and zero pollution. The development of hydrogen energy technology needs to focus on hydrogen production technology. Currently, fossil energy hydrogen production and industrial by-product hydrogen occupy the mainstream market, but both hydrogen production technologies have defects such as high carbon emissions and low hydrogen purity. Therefore, in the long run, water electrolysis is the most ideal way to produce hydrogen. Among them, the proton exchange membrane (PEM) water electrolysis hydrogen production technology generates oxygen and hydrogen by electrolyzing water. The water flows through the channel and diffusion layer in turn to the anode side of the proton exchange membrane. Under the action of the catalyst, electrolysis produces oxygen and hydrogen ions. Oxygen and water that does not participate in the electrolysis flow out of the electrolyzer through the channel, while hydrogen ions pass through the proton exchange membrane to the cathode side, combine with electrons to generate hydrogen, and flow into the hydrogen discharge channel through the cathode diffusion layer.
[0003] The PEM water electrolysis hydrogen production membrane electrode is the core component of the electrolyzer. It consists of three parts from the inside to the outside: the proton exchange membrane (PEM), the catalyst layer (CL) and the gas diffusion layer (GDL). It is the main place for material transmission and electrochemical reaction in the entire PEM electrolyzer. Among them, the catalyst layer provides a three-phase material transmission interface and an electrochemical reaction site, allowing the reaction gas, protons, and electrons to react on the electrocatalyst. The cathode catalyst layer and the anode catalyst layer are tightly attached to both sides of the proton exchange membrane, and the proton exchange membrane provides a transfer channel for protons from the anode to the cathode. The porous transport layer in the membrane electrode is usually in direct contact with the flow channel on the bipolar plate, playing the role of mechanical support, electron conduction, reaction gas diffusion and drainage.
[0004] The characteristics and structure of the membrane electrode will directly affect the performance and life of the PEM electrolyzer. Therefore, the preparation process of the PEM membrane electrode in the process of PEM water electrolysis to produce hydrogen is crucial to reducing the cost of the electrolysis system and improving the performance and life of the electrolyzer. The method is divided into CCS (Catalyst-coated substrate) method and CCM (Catalyst-oated membrane) The CCS method is to directly coat the catalyst active components on the GDL, prepare the cathode GDL and anode GDL coated with the catalyst layer, and then press the two GDLs on both sides of the PEM by hot pressing to obtain a membrane electrode. The more common method at this stage is the CCM method, which is to coat the catalyst active components on both sides of the PEM, and then directly attach the cathode GDL and anode GDL to the catalyst layers on both sides or hot press to obtain a membrane electrode.
[0005] The advantage of the CCS method for preparing PEM membrane electrodes is that its preparation process is relatively simple and mature, the preparation process is conducive to pore formation, and the proton exchange membrane will not swell and deform due to water absorption by the membrane; the disadvantage is that during the preparation process, the catalyst easily penetrates into the GDL, resulting in catalyst waste and reducing the utilization rate of the catalyst. In addition, the bonding force between the catalyst layer and the PEM is poor, and the interface resistance is large. The CCM method uses the core material of the PEM as a binder and directly coats the catalyst active components on both sides of the PEM, which will greatly reduce the proton transmission resistance between the PEM and the catalyst layer, and to a certain extent improve the performance of the membrane electrode and the utilization rate of the catalyst. However, in the prior art, during the use of the PEM membrane electrode, the proton exchange membrane is prone to swelling and deformation problems, and because the cathode and anode catalyst layers are mechanically bonded to the GDL, it will bring about the defect of large contact resistance, and the catalyst layer is easily impacted by circulating water and bubbles generated by electrolysis and falls off, thereby attenuating the electrochemical performance and reducing the service life. Summary of the invention
[0006] The present invention is mainly to overcome the defects of the prior art that the PEM membrane electrode is easy to swell and deform, and the contact resistance between the catalyst layer and the GDL is large when the PEM membrane electrode is prepared by the CCM method, and provides a membrane electrode assembly for hydrogen production by electrolysis of water by PEM and a preparation method thereof. The PEM membrane electrode assembly provided by the present invention can reduce the contact resistance between the catalyst layer and the GDL while enhancing the bonding force between the catalyst layer and the proton exchange membrane.
[0007] In a first aspect, the present invention provides a membrane electrode assembly for PEM water electrolysis to produce hydrogen, which comprises a cathode gas diffusion layer, a second cathode catalyst layer, a first cathode catalyst layer, a proton exchange membrane, a first anode catalyst layer, a second anode catalyst layer and an anode gas diffusion layer stacked in sequence;
[0008] The content of perfluorosulfonic acid ionomer in the second cathode catalyst layer is lower than that in the first cathode catalyst layer; the content of perfluorosulfonic acid ionomer in the second anode catalyst layer is lower than that in the first anode catalyst layer;
[0009] The loading amount of the active component in the first cathode catalyst layer and the first anode catalyst layer is not less than 0.01 mg / cm 2 The loading amount of the active component in the second cathode catalyst layer and the second anode catalyst layer is not less than 0.05 mg / cm 2 .
[0010] In the present invention, the catalyst loading refers to the amount of active ingredients per unit area of the membrane electrode, and can also be reflected in the thickness of the catalyst layer. When the concentration of the active ingredients in the slurry is the same, the greater the loading, the more active components per unit area of the membrane electrode, which can also indicate a greater thickness of the catalyst layer.
[0011] In the present invention, the test method for the active component loading in each catalyst layer is: tested in a Niton XL5 handheld spectrometer. The membrane electrode grid of the active component to be tested is divided into 10 areas, the Niton XL5 handheld spectrometer is turned on, the active component of the required test loading is set, and the instrument is calibrated with a standard sample. After the calibration is completed, each area to be measured is placed in the analysis chamber, and the test button is clicked for testing. After the analysis is completed, the handheld spectrometer will automatically generate an analysis report.
[0012] In the present invention, the content of the perfluorosulfonic acid ionomer in the first cathode catalyst layer and the first anode catalyst layer may be different.
[0013] In the present invention, the content of the perfluorosulfonic acid ionomer in the second cathode catalyst layer and the second anode catalyst layer may be different.
[0014] In the present invention, the first cathode catalyst layer, the second cathode catalyst layer, the first anode catalyst layer, and the second anode catalyst layer preferably all include active ingredients and perfluorosulfonic acid ionomers.
[0015] Among them, the active ingredient is preferably a platinum-based catalyst or an iridium-based catalyst; the platinum-based catalyst is preferably a Pt / C catalyst or a Pt-containing alloy catalyst; the Pt content in the Pt / C catalyst is preferably 10wt%-80wt%, for example 60wt%; the iridium-based catalyst is preferably one or more of iridium black, iridium oxide and iridium-containing alloy.
[0016] In some preferred embodiments, the active components in the first cathode catalyst layer and the second cathode catalyst layer are platinum-based catalysts.
[0017] In some preferred embodiments, the active component in the first anode catalyst layer and the second anode catalyst layer is an iridium-based catalyst.
[0018] In some specific embodiments, the active ingredient is a platinum-based catalyst, and the mass ratio of platinum in the platinum-based catalyst to the perfluorosulfonic acid ionomer may be 1:(0.1-10), such as 1:0.4, 1:0.45 or 1:0.5.
[0019] In some specific embodiments, the active ingredient is an iridium-based catalyst, and the mass ratio of iridium in the iridium-based catalyst to the perfluorosulfonic acid ionomer can be 1:(0.1-10), such as 1:0.25, 1:0.3 or 1:0.35.
[0020] In the present invention, based on the mass of the active components in the first cathode catalyst layer, the mass percentage of the perfluorosulfonic acid ionomer may be 10%-70%, preferably 20%-60%, for example 45%.
[0021] In the present invention, based on the mass of the active components in the second cathode catalyst layer, the mass percentage of the perfluorosulfonic acid ionomer may be 0%-60%, preferably 10%-50%, for example 0, 16% or 40%.
[0022] In the present invention, based on the mass of the active components in the first anode catalyst layer, the mass percentage of the perfluorosulfonic acid ionomer may be 10%-60%, preferably 20%-50%, for example 30%.
[0023] In the present invention, based on the mass of the active components in the second anode catalyst layer, the mass percentage of the perfluorosulfonic acid ionomer may be 0%-50%, preferably 10%-40%, for example 0, 10% or 25%.
[0024] In the present invention, the loading amount of the active component in the first anode catalyst layer is 0.01-5.0 mg / cm 2 , preferably 0.1-2 mg / cm 2 , for example 0.5 mg / cm 2 or 0.9mg / cm 2 .
[0025] In the present invention, the loading amount of the active component in the first cathode catalyst layer is 0.01-3.0 mg / cm 2 , preferably 0.1-1 mg / cm 2 , for example 0.3 mg / cm 2 or 0.4 mg / cm 2 .
[0026] In the present invention, the loading amount of the active component in the second anode catalyst layer is 0.05-5 mg / cm 2 , preferably 0.1-3.0 mg / cm 2 , for example 1mg / cm 2 or 0.1mg / cm 2 .
[0027] In the present invention, the loading amount of the active component in the second cathode catalyst layer is 0.05-3 mg / cm 2 , preferably 0.1-2.0 mg / cm 2 , for example 0.6 mg / cm 2 or 0.1mg / cm 2 .
[0028] In the present invention, the thickness of the proton exchange membrane can be conventional in the art, preferably 30-300 μm.
[0029] In the present invention, the material of the gas diffusion layer can be conventional in the art, and can be any one or more of titanium felt, titanium mesh, titanium foam, carbon cloth and carbon paper. The titanium felt is generally sintered titanium felt obtained through a sintering process.
[0030] In a second aspect, the present invention provides a method for preparing a membrane electrode assembly for PEM water electrolysis hydrogen production, which comprises the following steps: transferring a first catalyst layer to two surfaces of a proton exchange membrane, and then compounding it with a gas diffusion layer with a second catalyst layer to obtain the PEM membrane electrode;
[0031] The first catalyst layer includes a first anode catalyst layer and the first cathode catalyst layer, and the first anode catalyst layer and the first cathode catalyst layer are respectively loaded on both sides of the proton exchange membrane;
[0032] The gas diffusion layer with the second catalyst layer includes an anode gas diffusion layer with a second anode catalyst layer and a cathode gas diffusion layer with a second cathode catalyst layer. During the composite process, the second anode catalyst layer is in direct contact with the first anode catalyst layer; the second cathode catalyst layer is in direct contact with the first cathode catalyst layer;
[0033] The content of perfluorosulfonic acid ionomer in the second cathode catalyst layer is lower than that in the first cathode catalyst layer; the content of perfluorosulfonic acid ionomer in the second anode catalyst layer is lower than that in the first anode catalyst layer;
[0034] The loading amount of the active component in the first cathode catalyst layer and the first anode catalyst layer is not less than 0.01 mg / cm 2 The loading amount of the active component in the second cathode catalyst layer and the second anode catalyst layer is not less than 0.05 mg / cm 2 .
[0035] In the present invention, the transfer includes the following steps: loading the catalyst slurry on the base layer to form the first anode catalyst layer or the first cathode catalyst layer, then contacting the first anode catalyst layer or the first cathode catalyst layer with the proton exchange membrane, performing hot pressing, and then peeling off the base layer. The transfer operation can effectively overcome the problem of directly spraying or coating the catalyst layer on the proton exchange membrane, and the proton exchange membrane will swell and deform due to the influence of the base plate heating, solvent or temperature and humidity.
[0036] The loading method is preferably to spray the catalyst slurry onto the base layer.
[0037] Wherein, during the transfer process, the pressure of hot pressing is preferably 0.5-10 MPa, such as 1 MPa.
[0038] Wherein, during the transfer process, the temperature of the hot pressing is preferably 100°C-200°C, for example 180°C.
[0039] Wherein, in the transfer process, the heat pressing time is preferably 60s-300s, for example 200s;
[0040] The solvent of the catalyst slurry may optionally be water and / or alcohol, and the alcohol is preferably one or more of ethanol, isopropanol, n-propanol and ethylene glycol.
[0041] In the present invention, the method for preparing the gas diffusion layer with the second catalyst layer preferably includes the following steps: loading the second catalyst slurry on one side of the anode gas diffusion layer or the cathode gas diffusion layer by spraying or in-situ growth to form the second anode catalyst layer or the second cathode catalyst layer.
[0042] In some specific embodiments, the in situ growth includes the following steps: placing the anode gas diffusion layer or the cathode gas diffusion layer in a precursor solution of a catalyst active component, adjusting the pH to 11-14, reacting, and after the reaction is completed, cooling to 20-50°C, washing and drying to obtain the gas diffusion layer with a second catalyst layer.
[0043] Wherein, the solvent of the precursor solution is preferably a polyol, such as ethylene glycol.
[0044] Wherein, the solute of the precursor solution is preferably at least one of chloroiridic acid, chloroplatinic acid, ruthenium trichloride and chloroauric acid.
[0045] The precursor solution is preferably prepared by ultrasonic mixing for 1 hour.
[0046] The reaction temperature is preferably 120-160° C., and the reaction time is preferably 2-12 h.
[0047] The washing is performed with deionized water until no precipitation is found after titration with silver nitrate solution.
[0048] The drying method is preferably vacuum drying, and the drying temperature is preferably 50-80°C.
[0049] In the present invention, when the second catalyst layer is the second anode catalyst layer, the gas diffusion layer with the second catalyst layer can be heated and activated in a reducing atmosphere; the temperature of the heating activation is preferably 400°C-800°C; the reducing atmosphere is preferably any one of hydrogen, a mixture of hydrogen and nitrogen, argon, and helium; in the reducing atmosphere, the volume concentration of hydrogen is preferably 5-100%.
[0050] In the present invention, the compounding is preferably carried out under hot pressing conditions, the hot pressing pressure is preferably 0.1-5MPa, such as 0.8MPa; the hot pressing temperature is preferably 100℃-200℃, such as 160℃; the hot pressing time is preferably 60s-300s, such as 120s.
[0051] In the present invention, both the first catalyst layer and the second catalyst layer contain active components and perfluorosulfonic acid ionomer.
[0052] The perfluorosulfonic acid ionomer can be added in the form of a solution, and the concentration of the perfluorosulfonic acid ionomer in the solution is preferably 1wt%-70wt%, more preferably 1wt%-50wt%, further preferably 1wt%-40wt%, further more preferably 5wt%-30wt%, for example 5wt%.
[0053] Among them, the active ingredient is preferably a platinum-based catalyst and / or an iridium-based catalyst; the platinum-based catalyst is preferably a Pt / C catalyst or a Pt-containing alloy catalyst; the Pt content in the Pt / C catalyst is preferably 10wt%-80wt%; the iridium-based catalyst is preferably one or more of iridium powder, iridium oxide and iridium-containing alloy.
[0054] In some specific embodiments, the active ingredient is a platinum-based catalyst, and the mass ratio of platinum in the platinum-based catalyst to the perfluorosulfonic acid ionomer is preferably 1:(0.1-10), such as 1:0.4, 1:0.45 or 1:0.5.
[0055] In some specific embodiments, the active ingredient is an iridium-based catalyst, and the mass ratio of iridium in the iridium-based catalyst to the perfluorosulfonic acid ionomer is preferably 1:(0.1-10), such as 1:0.25, 1:0.3 or 1:0.35.
[0056] In the present invention, the loading amount of the active component in the first anode catalyst layer is 0.01-5.0 mg / cm 2 , preferably 0.1-2 mg / cm 2 , for example 0.5 mg / cm 2 or 0.9mg / cm 2 .
[0057] In the present invention, the loading amount of the active component in the first cathode catalyst layer is 0.01-3.0 mg / cm 2 , preferably 0.1-1 mg / cm 2 , for example 0.3 mg / cm 2 or 0.4 mg / cm 2 .
[0058] In the present invention, the loading amount of the active component in the second anode catalyst layer is 0.05-5 mg / cm 2 , preferably 0.1-3.0 mg / cm 2 , for example 1mg / cm 2 or 0.1mg / cm 2 .
[0059] In the present invention, the loading amount of the active component in the second cathode catalyst layer is 0.05-3 mg / cm 2 , preferably 0.1-2.0 mg / cm 2 , for example 0.6 mg / cm 2 or 0.1mg / cm 2 .
[0060] In the present invention, the material of the gas diffusion layer can be conventional in the art, and can be any one or more of titanium felt, titanium mesh, titanium foam, carbon cloth and carbon paper. The titanium felt is generally sintered titanium felt obtained through a sintering process.
[0061] In a third aspect, the present invention provides a membrane electrode assembly for PEM water electrolysis to produce hydrogen, which is prepared by the preparation method as described above.
[0062] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0063] The reagents and raw materials used in the present invention are commercially available.
[0064] The positive and progressive effects of the present invention are:
[0065] (1) In the structure of the membrane electrode assembly for PEM water electrolysis hydrogen production provided by the present invention, the first cathode and cathode catalyst layers are uniformly and tightly dispersed on the surface of the proton exchange membrane, and are glued to the cathode gas diffusion layer and the second cathode and cathode catalyst layers on the anode gas diffusion layer. The cathode and cathode catalyst layers adopt a gradient distribution structure of perfluorosulfonic acid ionomer to ensure that the "three-phase region" has enough catalytic active sites; at the same time, the contact resistance between the catalyst layer and the GDL layer can be reduced, which is beneficial to the transfer of electrons, protons and reactants, thereby further improving the electrochemical performance of the membrane electrode. Among them, when the voltage is 2V, the current density is increased by 17.2% compared with the CCM method, and increased by 54.5% compared with the CCM method, and the total catalyst loading can be reduced to less than 75% of the original CCM method.
[0066] (2) The preparation method of the membrane electrode assembly for PEM water electrolysis hydrogen production provided by the present invention prepares the membrane electrode by the catalyst layer transfer method, which largely overcomes the problem of swelling and deformation of the proton exchange membrane during the direct spraying and coating preparation of the proton exchange membrane by the influence of the bottom plate heating, solvent or laboratory temperature and humidity, thereby enhancing the bonding force between the catalyst layer and the proton exchange membrane;
[0067] At the same time, spraying or in-situ growing a gas diffusion layer with a second anion (cation) catalyst layer and then hot pressing it with the first anion (cation) catalyst layer effectively solves the problem of large contact impedance and large proton conduction resistance between the membrane electrode catalyst layer and the proton exchange membrane and the gas diffusion layer, and also reduces the conduction resistance of the external circuit electrons, which is conducive to proton capture of electrons; and further, it can reduce the loading of active components in the catalyst layer and improve the stability and durability of the catalyst layer. This preparation process can improve the electrochemical performance and stability of the PEM water electrolysis hydrogen production membrane electrode and reduce the catalyst loading. BRIEF DESCRIPTION OF THE DRAWINGS
[0068] Figure 1 A schematic diagram of the method for preparing a membrane electrode assembly for producing hydrogen through PEM water electrolysis provided by the present invention.
[0069] Figure 2 Schematic diagram of the preparation method of the membrane electrode assembly for PEM water electrolysis hydrogen production provided for Comparative Examples 1 and 2; wherein (a) is the CCS method; and (b) is the CCM method.
[0070] Figure 3 The polarization performance curves of the membrane electrode assemblies for producing hydrogen by electrolysis of water prepared in Example 1 and Comparative Examples 1-2 are shown.
[0071] Figure 4 The polarization performance curves of the membrane electrode assemblies for producing hydrogen by electrolysis of water prepared in Example 2 and Comparative Example 3 are shown. DETAILED DESCRIPTION
[0072] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0073] Example 1
[0074] (1) Preparation of proton exchange membrane: Cut a 6 cm × 6 cm Nafion115 proton exchange membrane, soak it in 5% H2O2 solution, 0.5 M H2SO4 solution, and deionized water at 80°C for 1 hour, then soak the washed proton exchange membrane in deionized water for later use. Dry the proton exchange membrane before use, and the active area is 5 cm × 5 cm;
[0075] Preparation of gas diffusion layer: Cut a piece of 5 cm × 5 cm carbon paper and sintered titanium felt, soak them in ethanol, ultrasonically clean them for 1 hour, and dry them for later use;
[0076] (2) uniformly dispersing a Pt / C cathode catalyst and a Nafion (perfluorosulfonic acid ionomer) solution in a solvent, and ultrasonically dispersing for 30 minutes to form a cathode catalyst slurry; wherein the Pt content in the Pt / C cathode catalyst is 60wt%; the concentration of Nafion in the Nafion solution is 5wt%; the solvent is a mixture of water and isopropanol in a volume ratio of 1:10; based on the total mass of the slurry, the proportion of the solvent is 30%;
[0077] According to the above method, cathode catalyst slurries with the mass of Nafion being 40%, 45% and 50% of the mass of Pt in the Pt / C cathode catalyst were prepared respectively;
[0078] Preparation of the first cathode catalyst layer: The three cathode catalyst slurries with different proportions were sprayed onto the transfer substrate PTFE in sequence by ultrasonic atomization spraying equipment. The Pt loading in the prepared first cathode catalyst layer was 0.4 mg / cm 2 ;
[0079] Preparation of the second cathode catalyst layer: The cathode catalyst slurry of the above Nafion with a mass of 40% of the mass of Pt in the Pt / C cathode catalyst is sprayed onto the carbon cloth through an ultrasonic atomization spraying device to prepare The second cathode catalyst layer The Pt loading is 0.1 mg / cm 2 ;
[0080] (3) The IrO2 anode catalyst and Nafion solution are uniformly dispersed in a solvent, and ultrasonic dispersion is performed for 30 minutes to form an anode catalyst slurry; wherein the concentration of Nafion in the Nafion solution is 5wt%; the solvent is a mixture of water and isopropanol in a volume ratio of 1:10; based on the total mass of the slurry, the proportion of the solvent is 30%;
[0081] According to the above method, anode catalyst slurries were prepared in which the mass of Nafion was 25%, 30%, and 35% of the mass of IrO2 anode catalyst respectively;
[0082] Preparation of the first anode catalyst layer: The three anode catalyst slurries with different proportions were sprayed onto the transfer substrate PTFE in sequence by ultrasonic atomization spraying equipment. The Ir loading in the prepared first anode catalyst layer was 0.9 mg / cm 2 ;
[0083] Preparation of the second anode catalyst layer: The anode catalyst slurry of the above Nafion with a mass of 25% of the mass of the IrO2 anode catalyst was sprayed onto the titanium felt by ultrasonic atomization spraying equipment. The Ir loading in the first and second anode catalyst layers was 0.1 mg / cm 2 ;
[0084] (4) The first cathode catalyst layer and the first anode catalyst layer are transferred to two opposite surfaces of the proton exchange membrane by hot pressing to form a CCM, wherein the hot pressing conditions are: 180° C., 1 MPa, and 200 s.
[0085] (5) The carbon paper with the second cathode catalyst layer prepared in step (2) is placed on the surface of the first cathode catalyst layer so that the catalyst layers are in direct contact, and the sintered titanium felt with the second anode catalyst layer prepared in step (3) is placed on the surface of the first anode catalyst layer so that the catalyst layers are in direct contact, and they are composited by hot pressing to prepare a membrane electrode assembly for hydrogen production by water electrolysis, the hot pressing temperature being 160°C, 0.8 MPa, and 120 s.
[0086] Example 2
[0087] (1) Preparation of proton exchange membrane: Cut a 6 cm × 6 cm Nafion115 proton exchange membrane, soak it in 5% H2O2 solution, 0.5 M H2SO4 solution, and deionized water at 80°C for 1 hour, then soak the washed proton exchange membrane in deionized water for later use. Dry the proton exchange membrane before use, and the active area is 5 cm × 5 cm;
[0088] Preparation of gas diffusion layer: Cut a piece of 5 cm × 5 cm carbon paper and sintered titanium felt, soak them in ethanol, ultrasonically clean them for 1 hour, and dry them for later use;
[0089] (2) Preparation of the first cathode catalyst layer: Pt / C cathode catalyst and Nafion solution were uniformly dispersed in a solvent, and ultrasonic dispersion was performed for 30 minutes to form a cathode catalyst slurry; wherein the Pt content in the Pt / C cathode catalyst was 60wt%; the concentration of Nafion in the Nafion solution was 5wt%; the solvent was a mixture of water and isopropanol in a volume ratio of 1:10; based on the total mass of the slurry, the proportion of the solvent was 30%;
[0090] According to the above method, cathode catalyst slurries with the mass of Nafion being 40%, 45% and 50% of the mass of Pt in the Pt / C cathode catalyst were prepared respectively;
[0091] The three cathode catalyst slurries with different proportions were sprayed onto the transfer substrate PTFE in sequence by ultrasonic atomization spraying equipment. The Pt loading in the first cathode catalyst layer was 0.4 mg / cm 2 ;
[0092] (3) Preparation of the second cathode catalyst layer:
[0093] 1) preparing a chloroplatinic acid (Aladdin) ethylene glycol precursor solution, wherein the concentration of the chloroplatinic acid is 1 wt %, and ultrasonically mixing for 1 hour;
[0094] 2) placing the non-hydrophobic carbon paper in the ethylene glycol precursor solution prepared in 1), heating to 150° C., and magnetically stirring;
[0095] 3) titrating sodium hydroxide solution to adjust the pH value of the solution to 14, and the reaction time is 12 hours;
[0096] 4) Cooling to 20-50° C., taking out the carbon paper carrying the second cathode catalyst layer, and washing it with deionized water until there is no precipitation when the silver nitrate solution is titrated;
[0097] 5) After washing, the mixture was dried in a vacuum oven at 60°C to obtain a cathode gas diffusion layer loaded with a second cathode diffusion layer, wherein the Pt loading was 0.1 mg / cm 2 ;
[0098] (4) Preparation of the first anode catalyst layer: IrO2 anode catalyst and Nafion solution were uniformly dispersed in a solvent, and ultrasonic dispersion was performed for 30 minutes to form an anode catalyst slurry; wherein the concentration of Nafion in the Nafion solution was 5wt%; the solvent was a mixture of water and isopropanol in a volume ratio of 1:10; based on the total mass of the slurry, the proportion of the solvent was 30%;
[0099] According to the above method, anode catalyst slurries with a mass of Nafion of 25%, 30%, and 35% of the mass of IrO2 anode catalyst were prepared respectively; the above three different proportions of anode catalyst slurries were sprayed onto the transfer substrate PTFE in sequence by ultrasonic atomization spraying equipment, and the total Ir loading in the first anode catalyst layer was 0.9 mg / cm 2 ;
[0100] (5) Preparation of the second anode catalyst layer:
[0101] 1) preparing an ethylene glycol solution of chloroiridic acid, wherein the concentration of chloroiridic acid is 0.6 wt %, and ultrasonically mixing for 1 hour;
[0102] 2) placing the titanium felt in the ethylene glycol solution obtained in step 1), heating the solution to 160° C., and stirring with a magnetic stirrer;
[0103] 3) adding sodium hydroxide solution to adjust the pH value of the solution in step 2) to 14, and the reaction time is 6 hours;
[0104] 4) Cooling to room temperature, taking out the titanium felt with the second anode catalyst layer, and washing it with deionized water until there is no precipitation when the silver nitrate solution is titrated;
[0105] 5) After washing, dry in a vacuum oven at 60°C;
[0106] 6) The titanium felt with the material obtained in step 5) is heated and activated in an argon atmosphere at a temperature range of 400-800°C for 2 hours to obtain an anode gas diffusion layer loaded with a second anode diffusion layer; wherein the Ir loading is 0.1 mg / cm 2 ;
[0107] (6) The first cathode catalyst layer prepared in step (2) and the first anode catalyst layer prepared in step (4) are transferred to two opposite surfaces of the proton exchange membrane by hot pressing to form a CCM. The hot pressing conditions are: 180° C., 1 MPa, and 200 s.
[0108] (7) The carbon paper with the second cathode catalyst layer prepared in step (3) is placed on the surface of the first cathode catalyst layer so that the catalyst layers are in direct contact, and the titanium felt with the second anode catalyst layer prepared in step (5) is placed on the surface of the first anode catalyst layer so that the catalyst layers are in direct contact, and they are composited by hot pressing to prepare a membrane electrode assembly for hydrogen production by PEM water electrolysis; the hot pressing temperature is 160°C, 0.8MPa, and 120s.
[0109] Example 3
[0110] (1) Preparation of proton exchange membrane: Cut a 6 cm × 6 cm Nafion115 proton exchange membrane, soak it in 5% H2O2 solution, 0.5 M H2SO4 solution, and deionized water at 80°C for 1 hour, then soak the washed proton exchange membrane in deionized water for later use. Dry the proton exchange membrane before use, and the active area is 5 cm × 5 cm;
[0111] Preparation of gas diffusion layer: Cut a piece of 5 cm × 5 cm carbon paper and sintered titanium felt, soak them in ethanol, ultrasonically clean them for 1 hour, and dry them for later use;
[0112] (2) uniformly dispersing a Pt / C cathode catalyst and a Nafion (perfluorosulfonic acid ionomer) solution in a solvent, and ultrasonically dispersing for 30 minutes to form a cathode catalyst slurry; wherein the Pt content in the Pt / C cathode catalyst is 60wt%; the concentration of Nafion in the Nafion solution is 5wt%; the solvent is a mixture of water and isopropanol in a volume ratio of 1:10; based on the total mass of the slurry, the proportion of the solvent is 30%;
[0113] According to the above method, cathode catalyst slurries with the mass of Nafion being 40%, 45% and 50% of the mass of Pt in the Pt / C cathode catalyst were prepared respectively;
[0114] Preparation of the first cathode catalyst layer: The three cathode catalyst slurries with different proportions were sprayed onto the transfer substrate PTFE in sequence by ultrasonic atomization spraying equipment. The Pt loading in the prepared first cathode catalyst layer was 0.4 mg / cm 2 ;
[0115] Preparation of the second cathode catalyst layer: The cathode catalyst slurry with a mass of Nafion of 16% of the mass of Pt in the Pt / C cathode catalyst was sprayed onto the carbon cloth by ultrasonic atomization spraying equipment. The Pt loading in the prepared second cathode catalyst layer was 0.1 mg / cm 2 ;
[0116] (3) The IrO2 anode catalyst and Nafion solution are uniformly dispersed in a solvent, and ultrasonic dispersion is performed for 30 minutes to form an anode catalyst slurry; wherein the concentration of Nafion in the Nafion solution is 5wt%; the solvent is a mixture of water and isopropanol in a volume ratio of 1:10; based on the total mass of the slurry, the proportion of the solvent is 30%;
[0117] According to the above method, anode catalyst slurries were prepared in which the mass of Nafion was 25%, 30%, and 35% of the mass of IrO2 anode catalyst respectively;
[0118] Preparation of the first anode catalyst layer: The three anode catalyst slurries with different proportions were sprayed onto the transfer substrate PTFE in sequence by ultrasonic atomization spraying equipment. The Ir loading in the prepared first anode catalyst layer was 0.9 mg / cm 2 ;
[0119] Preparation of the second anode catalyst layer: The anode catalyst slurry of the above Nafion with a mass of 10% of the mass of the IrO2 anode catalyst was sprayed onto the titanium felt by ultrasonic atomization spraying equipment. The Ir loading in the first and second anode catalyst layers was 0.1 mg / cm 2 ;
[0120] (4) The first cathode catalyst layer and the first anode catalyst layer are transferred to two opposite surfaces of the proton exchange membrane by hot pressing to form a CCM, wherein the hot pressing conditions are: 180° C., 1 MPa, and 200 s.
[0121] (5) The carbon paper with the second cathode catalyst layer prepared in step (2) is placed on the surface of the first cathode catalyst layer so that the catalyst layers are in direct contact, and the sintered titanium felt with the second anode catalyst layer prepared in step (3) is placed on the surface of the first anode catalyst layer so that the catalyst layers are in direct contact, and they are composited by hot pressing to prepare a membrane electrode assembly for hydrogen production by water electrolysis, the hot pressing temperature being 160°C, 0.8 MPa, and 120 s.
[0122] Comparative Example 1
[0123] (1) Preparation of proton exchange membrane: Cut a 6 cm × 6 cm Nafion115 proton exchange membrane, soak it in 5% H2O2 solution, 0.5 M H2SO4 solution, and deionized water at 80°C for 1 hour, then soak the washed proton exchange membrane in deionized water for later use. Dry the proton exchange membrane before use, and the active area is 5 cm × 5 cm;
[0124] Preparation of gas diffusion layer: Cut a piece of 5 cm × 5 cm carbon paper and sintered titanium felt, soak them in ethanol, ultrasonically clean them for 1 hour, and dry them for later use;
[0125] (2) uniformly dispersing the Pt / C cathode catalyst and the Nafion solution in a solvent, and ultrasonically dispersing for 30 minutes to form a cathode catalyst slurry; wherein the Pt content in the Pt / C cathode catalyst is 60wt%; the concentration of Nafion in the Nafion solution is 5wt%; the solvent is a mixture of water and isopropanol in a volume ratio of 1:10; based on the total mass of the slurry, the proportion of the solvent is 30%;
[0126] According to the above method, a cathode catalyst slurry with a mass of Nafion of 45% of the mass of Pt in the Pt / C cathode catalyst was prepared; the cathode catalyst slurry was sprayed onto the proton exchange membrane by ultrasonic atomization spraying equipment to obtain a cathode catalyst layer, in which the Pt loading amount was 0.5 mg / cm 2 ;
[0127] (3) The IrO2 anode catalyst and Nafion solution are uniformly dispersed in a solvent, and ultrasonic dispersion is performed for 30 minutes to form an anode catalyst slurry; wherein the concentration of Nafion in the Nafion solution is 5wt%; the solvent is a mixture of water and isopropanol in a volume ratio of 1:10; based on the total mass of the slurry, the proportion of the solvent is 30%;
[0128] According to the above method, an anode catalyst slurry with a mass of Nafion of 30% of the mass of IrO2 anode catalyst was prepared; the anode catalyst slurry was sprayed onto the proton exchange membrane by ultrasonic atomization spraying equipment to obtain an anode catalyst layer, in which the Ir loading amount was 1 mg / cm 2 ;
[0129] (4) The cathode catalyst layer and the anode catalyst layer are transferred to the two opposite sides of the proton exchange membrane by hot pressing, and the carbon paper and sintered titanium felt are bonded to the anode and cathode catalyst layers by hot pressing to form a gas diffusion layer, and a membrane electrode assembly for hydrogen production by PEM water electrolysis is prepared at the same time. The hot pressing temperature is 180°C, 1MPa, and 200s.
[0130] Comparative Example 2
[0131] (1) Preparation of proton exchange membrane: Cut a 6 cm × 6 cm Nafion115 proton exchange membrane, soak it in 5% H2O2 solution, 0.5 M H2SO4 solution, and deionized water at 80°C for 1 hour, then soak the washed proton exchange membrane in deionized water for later use. Dry the proton exchange membrane before use, and the active area is 5 cm × 5 cm;
[0132] Preparation of gas diffusion layer: Cut a piece of 5 cm × 5 cm carbon paper and sintered titanium felt, soak them in ethanol, ultrasonically clean them for 1 hour, and dry them for later use;
[0133] (2) uniformly dispersing the Pt / C cathode catalyst and the Nafion solution in a solvent, and ultrasonically dispersing for 30 minutes to form a cathode catalyst slurry; wherein the Pt content in the Pt / C cathode catalyst is 60wt%; the concentration of Nafion in the Nafion solution is 5wt%; the solvent is a mixture of water and isopropanol in a volume ratio of 1:10; based on the total mass of the slurry, the proportion of the solvent is 30%;
[0134] According to the above method, a cathode catalyst slurry with a mass of Nafion of 45% of the mass of Pt in the Pt / C cathode catalyst was prepared; the cathode catalyst slurry was sprayed onto carbon paper by ultrasonic atomization spraying equipment to obtain a cathode catalyst layer, in which the Pt loading amount was 0.5 mg / cm 2 ;
[0135] (3) The IrO2 anode catalyst and Nafion solution are uniformly dispersed in a solvent, and ultrasonic dispersion is performed for 30 minutes to form an anode catalyst slurry; wherein the concentration of Nafion in the Nafion solution is 5wt%; the solvent is a mixture of water and isopropanol in a volume ratio of 1:10; based on the total mass of the slurry, the proportion of the solvent is 30%;
[0136] According to the above method, an anode catalyst slurry with a mass of Nafion of 30% of the mass of IrO2 anode catalyst was prepared; the anode catalyst slurry was sprayed onto a sintered titanium felt by ultrasonic atomization spraying equipment to obtain an anode catalyst layer, wherein the Ir loading amount was 1 mg / cm 2 ;
[0137] (4) Carbon paper loaded with a cathode catalyst layer and sintered titanium felt loaded with an anode catalyst layer are respectively placed on the surface of a proton exchange membrane for compounding by hot pressing, wherein the catalyst layer is in direct contact with the proton exchange membrane, to prepare a membrane electrode assembly for hydrogen production by PEM water electrolysis, the hot pressing temperature is 180°C, 1MPa, and 200s.
[0138] Comparative Example 3
[0139] (1) Preparation of proton exchange membrane: Cut a 6 cm × 6 cm Nafion115 proton exchange membrane, soak it in 5% H2O2 solution, 0.5 M H2SO4 solution, and deionized water at 80°C for 1 hour, then soak the washed proton exchange membrane in deionized water for later use. Dry the proton exchange membrane before use, and the active area is 5 cm × 5 cm;
[0140] Preparation of gas diffusion layer: Cut a piece of 5 cm × 5 cm carbon paper and sintered titanium felt, soak them in ethanol, ultrasonically clean them for 1 hour, and dry them for later use;
[0141] (2) uniformly dispersing the Pt / C cathode catalyst and the Nafion solution in a solvent, and ultrasonically dispersing for 30 minutes to form a cathode catalyst slurry; wherein the Pt content in the Pt / C cathode catalyst is 60wt%; the concentration of Nafion in the Nafion solution is 5wt%; the solvent is a mixture of water and isopropanol in a volume ratio of 1:10; based on the total mass of the slurry, the proportion of the solvent is 30%;
[0142] According to the above method, a cathode catalyst slurry with a mass of Nafion of 50% of the mass of Pt in the Pt / C cathode catalyst was prepared; the cathode catalyst slurry was sprayed onto the transfer substrate PTFE by ultrasonic atomization spraying equipment to obtain a cathode catalyst layer, in which the Pt loading amount was 0.5 mg / cm 2 ;
[0143] (3) The anode catalyst IrO2 and 5% Nafion solution were uniformly dispersed in water and isopropanol solvents, and ultrasonic dispersion was performed for 30 min to form an anode catalyst slurry. The slurry was sprayed onto the transfer substrate PTFE by ultrasonic atomization spraying equipment. The dry Nafion mass was 40% of the Ir mass, and the Ir loading was 1 mg / cm 2 ;
[0144] (4) The cathode catalyst layer and the anode catalyst layer are transferred to two opposite surfaces of the proton exchange membrane by hot pressing, and the carbon paper and sintered titanium felt are bonded to the anode and cathode catalyst layers by hot pressing to form a gas diffusion layer, thereby obtaining a membrane electrode assembly for hydrogen production by water electrolysis of PEM, the hot pressing temperature is 180°C, 1MPa, and 200s.
[0145] Table 1
[0146]
[0147]
[0148] Effect Example
[0149] 1. Polarization performance test
[0150] The membrane electrode prepared in the embodiment and the comparative example was assembled into a PEM water electrolysis test system for polarization performance test. The test temperature was 50°C and the active area of the test membrane electrode was 25 cm 2 The test results are shown in Table 2.
[0151] 2. Contact resistance
[0152] The membrane electrodes prepared in the embodiments and comparative examples were subjected to contact resistance tests. The tests were performed using a HIOKI-BT3564 contact resistance tester. The test results are shown in Table 2.
[0153] Table 2
[0154]
[0155] The present invention is based on Figure 1 The schematic diagram of the preparation method of the membrane electrode assembly for PEM water electrolysis hydrogen production is shown. The contact resistance of the membrane electrode assembly for PEM water electrolysis hydrogen production can be less than 100mΩ·cm through the above-mentioned specific embodiments.2 Furthermore, when the precious metal loading is the same, a lower voltage can be achieved at the same current density; and a higher current density can be achieved at the same voltage, which proves that the performance of the membrane electrode provided by the present invention is greatly improved.
[0156] Comparative Example 1 adopted the CCM method. Figure 2 Part (b) of FIG. 1 shows the preparation process. It can be seen that the difference between Comparative Example 1 and Example 1 is that the cathode (anode) catalyst layer in Comparative Example 1 has only one layer and is directly sprayed on both sides of the proton exchange membrane. Figure 3 It can be seen that when the voltage is 2.0V, the membrane electrode current density of Example 1 is 3.4A / cm 2 The membrane electrode current density of comparative example 1 is 2.9A / cm 2 , lower than Example 1, and its contact resistance is greater than Example 1. This may be due to the fact that Example 1 adopts a gradient design of perfluorosulfonic acid ionomer and catalyst, the high content of Nafion in the first catalyst layer on the proton exchange membrane side improves the proton conduction between the membrane and the catalyst layer, and the membrane electrode preparation method combining CCM and CCS improves the electronic conduction between the catalyst layer and the gas diffusion layer. Therefore, the membrane electrode contact resistance of Example 1 is significantly reduced, and the membrane electrode electrochemical performance is more superior.
[0157] Comparative Example 2 adopted the CCS method. Figure 2 Part (a) of FIG. 2 shows the preparation process. It can be seen that the difference between Comparative Example 2 and Example 1 is that the cathode (anode) catalyst layer of Comparative Example 2 has only one layer and is directly sprayed on both sides of the gas diffusion layer. Figure 3 It can be seen that when the voltage is 2.0V, the membrane electrode current density of Example 1 is 3.4A / cm 2 The membrane electrode current density of comparative example 2 is 2.2A / cm 2 , which is lower than that in Example 1, and its contact resistance is much greater than that in Example 1. This may be because the poor bonding between the catalyst layer and the proton exchange membrane results in a large interface resistance, which affects the transmission of protons and electrons and reduces the current density.
[0158] The difference between Comparative Example 3 and Example 1 is that the cathode (anode) catalyst layer in Comparative Example 3 has only one layer and the gas diffusion layer is not loaded with a catalyst layer. Figure 4 It can be seen from the data that the current density is 1 or 2A / cm 2When the voltage of Example 1 is less than that of Comparative Example 3, its contact resistance is much greater than that of Example 1. This may be because Example 1 adopts a membrane electrode preparation method combining CCM and CCS, which improves the electronic conduction of the catalyst layer and the gas diffusion layer. The dry Nafion content in the cathode and anode catalyst layers in Comparative Example 3 is higher than that in Example 1. Although it can improve its proton conduction ability, the porosity in the catalyst layer also decreases, which is not conducive to the transmission of gas and water. Therefore, the electrochemical performance of the membrane electrode of Example 1 is more superior.
[0159] Example 2 adopts two methods, spraying and in-situ growth, to prepare the first cathode (anode) catalyst layer and the second cathode (anode) catalyst layer respectively. Figure 4 It can be seen from the data that a lower contact resistance can be obtained, and a lower voltage can be obtained when the current density is the same.
[0160] The difference between Examples 1-3 is that the perfluorosulfonic acid ionomers in the anode and cathode catalyst layers are distributed in a gradient manner using different proportions. Experiments have shown that the perfluorosulfonic acid ionomer distribution structure with a suitable proportion can significantly reduce the contact resistance between the catalyst layer and the GDL layer, thereby improving the electrochemical performance of the membrane electrode.
[0161] The embodiments described above are only some embodiments of the present invention, which are convenient for those skilled in the art to understand and use the present invention. Obviously, any person skilled in the art can slightly modify or change the present embodiment and apply it to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and any equal changes, simple modifications and modifications made within the scope of the present invention still belong to the scope of the present invention.
Claims
1. A membrane electrode assembly for PEM water electrolysis to produce hydrogen, characterized in that: It comprises a cathode gas diffusion layer, a second cathode catalyst layer, a first cathode catalyst layer, a proton exchange membrane, a first anode catalyst layer, a second anode catalyst layer and an anode gas diffusion layer which are stacked in sequence; The content of perfluorosulfonic acid ionomer in the second cathode catalyst layer is lower than that in the first cathode catalyst layer; the content of perfluorosulfonic acid ionomer in the second anode catalyst layer is lower than that in the first anode catalyst layer; The loading amount of the active component in the first cathode catalyst layer and the first anode catalyst layer is not less than 0.01 mg / cm 2 The loading amount of the active component in the second cathode catalyst layer and the second anode catalyst layer is not less than 0.05 mg / cm 2 .
2. The membrane electrode assembly for producing hydrogen by PEM water electrolysis according to claim 1, characterized in that: The first cathode catalyst layer and the first anode catalyst layer have different contents of perfluorosulfonic acid ionomer; and / or, the content of perfluorosulfonic acid ionomer in the second cathode catalyst layer is different from that in the second anode catalyst layer; and / or, based on the mass of the active components in the first cathode catalyst layer, the mass percentage of the perfluorosulfonic acid ionomer is 10%-70%, preferably 20%-60%, for example 45%; and / or, based on the mass of the active component in the second cathode catalyst layer, the mass percentage of the perfluorosulfonic acid ionomer is 0%-60%, preferably 10%-50%, for example 0, 16% or 40%; and / or, based on the mass of the active components in the first anode catalyst layer, the mass percentage of the perfluorosulfonic acid ionomer is 10%-60%, preferably 20%-50%, for example 30%; And / or, based on the mass of the active components in the second anode catalyst layer, the mass percentage of the perfluorosulfonic acid ionomer is 0%-50%, preferably 10%-40%, for example 0, 10% or 25%.
3. The membrane electrode assembly for producing hydrogen by PEM water electrolysis according to claim 1, characterized in that: The active component is a platinum-based catalyst or an iridium-based catalyst; the platinum-based catalyst is preferably a Pt / C catalyst or a Pt-containing alloy catalyst; the Pt content in the Pt / C catalyst is preferably 10wt%-80wt%, for example 60wt%; the iridium-based catalyst is preferably one or more of iridium black, iridium oxide and an iridium-containing alloy; preferably, the active component in the first cathode catalyst layer and the second cathode catalyst layer is a platinum-based catalyst; preferably, the active component in the first anode catalyst layer and the second anode catalyst layer is an iridium-based catalyst; And / or, in the first anode catalyst layer, the loading amount of the active component is 0.01-5.0 mg / cm 2 , preferably 0.1-2 mg / cm 2 , for example 0.5 mg / cm 2 or 0.9mg / cm 2 ; And / or, in the first cathode catalyst layer, the loading amount of the active component is 0.01-3.0 mg / cm 2 , preferably 0.1-1 mg / cm 2 , for example 0.3 mg / cm 2 or 0.4mg / cm 2 ; And / or, in the second anode catalyst layer, the loading amount of the active ingredient is 0.05-5 mg / cm 2 , preferably 0.1-3.0 mg / cm 2 , for example 1mg / cm 2 or 0.1mg / cm 2 ; And / or, in the second cathode catalyst layer, the loading amount of the active component is 0.05-3 mg / cm 2 , preferably 0.1-2.0 mg / cm 2 , for example 0.6 mg / cm 2 or 0.1mg / cm 2 .
4. The membrane electrode assembly for producing hydrogen by PEM water electrolysis according to claim 1, characterized in that: The active ingredient is a platinum-based catalyst, and the mass ratio of platinum in the platinum-based catalyst to the perfluorosulfonic acid ionomer is 1:(0.1-10), such as 1:0.4, 1:0.45 or 1:0.5; And / or, the active ingredient is an iridium-based catalyst, and the mass ratio of iridium in the iridium-based catalyst to the perfluorosulfonic acid ionomer is 1:(0.1-10), such as 1:0.25, 1:0.3 or 1:0.35; and / or, the first cathode catalyst layer, the second cathode catalyst layer, the first anode catalyst layer, and the second anode catalyst layer all include active ingredients and perfluorosulfonic acid ionomer; And / or, the thickness of the proton exchange membrane is 30-300 μm; And / or, the material of the gas diffusion layer is any one or more of titanium felt, titanium mesh, titanium foam, carbon cloth and carbon paper.
5. A method for preparing a membrane electrode assembly for PEM water electrolysis hydrogen production, characterized in that: The method comprises the following steps: transferring the first catalyst layer to two surfaces of the proton exchange membrane, and then compounding the first catalyst layer with the gas diffusion layer having the second catalyst layer to obtain the PEM membrane electrode; Wherein, the first catalyst layer comprises a first anode catalyst layer and the first cathode catalyst layer, and the first anode catalyst layer and the first cathode catalyst layer are respectively loaded on both sides of the proton exchange membrane; The gas diffusion layer with the second catalyst layer comprises an anode gas diffusion layer with a second anode catalyst layer and a cathode gas diffusion layer with a second cathode catalyst layer. During the composite process, the second anode catalyst layer is in direct contact with the first anode catalyst layer; the second cathode catalyst layer is in direct contact with the first cathode catalyst layer; The content of perfluorosulfonic acid ionomer in the second cathode catalyst layer is lower than that in the first cathode catalyst layer; the content of perfluorosulfonic acid ionomer in the second anode catalyst layer is lower than that in the first anode catalyst layer; the loading amount of active components in the first cathode catalyst layer and the first anode catalyst layer is not less than 0.01 mg / cm 2 The loading amount of the active component in the second cathode catalyst layer and the second anode catalyst layer is not less than 0.05 mg / cm 2 .
6. The method for preparing a membrane electrode assembly for producing hydrogen by PEM water electrolysis according to claim 5, characterized in that: The transfer comprises the following steps: loading the catalyst slurry on the base layer to form the first anode catalyst layer or the first cathode catalyst layer, then contacting the first anode catalyst layer or the first cathode catalyst layer with the proton exchange membrane, performing hot pressing, and then peeling off the base layer; Wherein, the pressure of the hot pressing is preferably 0.5-10MPa, for example 1MPa; Wherein, the temperature of the hot pressing is preferably 100°C-200°C, for example 180°C; Wherein, the heat pressing time is preferably 60s-300s, for example 200s; The solvent of the catalyst slurry may optionally be water and / or alcohol, and the alcohol is preferably one or more of ethanol, isopropanol, n-propanol and ethylene glycol.
7. The method for preparing a membrane electrode assembly for producing hydrogen by PEM water electrolysis according to claim 5, characterized in that: The method for preparing the gas diffusion layer with the second catalyst layer comprises the following steps: loading the second catalyst slurry on one side of the anode gas diffusion layer or the cathode gas diffusion layer by spraying or in-situ growth to form the second anode catalyst layer or the cathode catalyst layer; Wherein, the in-situ growth preferably includes the following steps: placing the anode gas diffusion layer or the cathode gas diffusion layer in a precursor solution of a catalyst active component, adjusting the pH to 11-14, reacting, cooling to 20-50°C after the reaction, washing and drying, so as to obtain the gas diffusion layer with the second catalyst layer; the solvent of the precursor solution is preferably a polyol, such as ethylene glycol; the solute of the precursor solution is preferably at least one of chloroiridic acid, chloroplatinic acid, ruthenium trichloride and chloroauric acid; the preparation of the precursor solution is preferably carried out by ultrasonic mixing for 1 hour; the reaction temperature is preferably 120-160°C; the reaction time is preferably 2-12 hours; the drying method is preferably vacuum drying, and the drying temperature is preferably 50-80°C; Wherein, when the second catalyst layer is the second anode catalyst layer, the gas diffusion layer with the second catalyst layer is heated and activated in a reducing atmosphere; the temperature of the heating activation is preferably 400°C-800°C; the reducing atmosphere is preferably any one of hydrogen, a mixture of hydrogen and nitrogen, argon, and helium; in the reducing atmosphere, the volume concentration of hydrogen is preferably 5-100%.
8. The method for preparing a membrane electrode assembly for producing hydrogen by PEM water electrolysis according to claim 5, characterized in that: The compounding is carried out under hot pressing conditions, wherein the hot pressing pressure is preferably 0.1-5MPa, such as 0.8MPa; the hot pressing temperature is preferably 100°C-200°C, such as 160°C; and the hot pressing time is preferably 60s-300s, such as 120s.
9. The method for preparing a membrane electrode assembly for producing hydrogen by PEM water electrolysis according to claim 5, characterized in that: The perfluorosulfonic acid ionomer is added in the form of a solution, wherein the concentration of the perfluorosulfonic acid ionomer in the solution is 1wt%-70wt%, preferably 1wt%-50wt%, more preferably 1wt%-40wt%, further more preferably 5wt%-30wt%, for example 5wt%; And / or, the active ingredient is a platinum-based catalyst and / or an iridium-based catalyst; the platinum-based catalyst is preferably a Pt / C catalyst or a Pt-containing alloy catalyst; the Pt content in the Pt / C catalyst is preferably 10wt%-80wt%, for example 60wt%; the iridium-based catalyst is preferably one or more of iridium powder, iridium oxide and iridium-containing alloy; And / or, the active ingredient is a platinum-based catalyst, and the mass ratio of platinum in the platinum-based catalyst to the perfluorosulfonic acid ionomer is preferably 1:(0.1-10), such as 1:0.4, 1:0.45 or 1:0.5; And / or, the active ingredient is an iridium-based catalyst, and the mass ratio of iridium in the iridium-based catalyst to the perfluorosulfonic acid ionomer is preferably 1:(0.1-10), such as 1:0.25, 1:0.3 or 1:0.35; And / or, in the first anode catalyst layer, the loading amount of the active component is 0.01-5.0 mg / cm 2 , preferably 0.1-2 mg / cm 2 , for example 0.5 mg / cm 2 or 0.9mg / cm 2 ; And / or, in the first cathode catalyst layer, the loading amount of the active component is 0.01-3.0 mg / cm 2 , preferably 0.1-1 mg / cm 2 , for example 0.3 mg / cm 2 or 0.4mg / cm 2 ; And / or, in the second anode catalyst layer, the loading amount of the active ingredient is 0.05-5 mg / cm 2 , preferably 0.1-3.0 mg / cm 2 , for example 1mg / cm 2 or 0.1mg / cm 2 ; And / or, in the second cathode catalyst layer, the loading amount of the active component is 0.05-3 mg / cm 2 , preferably 0.1-2.0 mg / cm 2 , for example 0.6 mg / cm 2 or 0.1mg / cm 2 ; And / or, the material of the gas diffusion layer is any one or more of titanium felt, titanium mesh, titanium foam, carbon cloth and carbon paper.
10. A membrane electrode assembly for PEM water electrolysis to produce hydrogen, which is prepared by the preparation method according to any one of claims 5 to 9.
Citation Information
Cited By
Anode electrode, preparation method of anode electrode, membrane electrode and application of membrane electrode
CN119776875A
Proton exchange membrane electrolyzed water membrane electrode with catalyst layer constructed by mixed ionomers and preparation method of proton exchange membrane electrolyzed water membrane electrode
CN120006312A
A proton exchange membrane water electrolysis membrane electrode with a mixed ionomer constructed catalytic layer and a preparation method thereof
CN120006312B
Device for hydrogen production by electrolysis
TWI912234B