Anti-purple light semitransparent organic photovoltaic device structure and preparation method thereof

By designing and integrating the UV filter layer prepared by alternating evaporation of LiF and TeO2 in semi-transparent organic photovoltaic devices, the problem of ultraviolet light protection not considered in the prior art is solved, and filtering of ultraviolet light below 380nm wavelength is achieved. Improves the security and performance of the device and promotes its commercial applications.

CN119031735APending Publication Date: 2024-11-26SHANDONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411076474.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing translucent organic photovoltaic device structure does not consider the light protection design of ultraviolet light, resulting in the impact of ultraviolet transmission on the human body that has not been evaluated and resolved, affecting its large-scale commercial application.

Method used

A UV filter layer compatible with the experimental process was designed. The UV filter layer was prepared by alternating evaporation of LiF and TeO2, filtering ultraviolet light below 380nm wavelength, and integrating it into semi-transparent organic photovoltaic devices to avoid transmission of the device. Reduced rate and complicated process.

Benefits of technology

It effectively improves the ultraviolet light protection capability of the device, maintains the photoelectric performance and visible light transmittance of translucent photovoltaic devices, reduces the threat of ultraviolet light to the human body, and provides photobiological security guarantees for its large-scale commercial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119031735A_ABST
    Figure CN119031735A_ABST
Patent Text Reader

Abstract

The invention relates to an anti-purple-light semitransparent organic photovoltaic device structure and a preparation method thereof. The anti-purple-light semitransparent organic photovoltaic device structure comprises a substrate, an anode, a hole transport layer, an active layer, an electron transport layer, a cathode and a UV filter layer which are sequentially grown from bottom to top. According to the invention, the 380nm high-wave-pass optical filter is selected and added to the metal cathode, so that the performance of the device is not reduced, and meanwhile, the ultraviolet light in the transmission spectrum of the device is effectively reduced. After the ultraviolet light is filtered by the UV optical filter, the corresponding safe exposure time of the device reaches an exemption level, and the light safety problem caused by the ultraviolet light is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a UV-proof semi-transparent organic photovoltaic device structure and a preparation method thereof, belonging to the technical field of organic photovoltaic device preparation. Background Art

[0002] Semi-transparent organic photovoltaics have attracted widespread attention due to their applications in building photovoltaic integration, smart windows, agricultural greenhouses and other fields. Driven by many researchers, the light energy utilization rate of this type of equipment has exceeded 5%, and large-scale commercial applications are just around the corner. However, the research on light safety of semi-transparent photovoltaics has not received much attention from researchers, which is an inevitable and important link for the large-scale application of semi-transparent photovoltaic devices. A large number of medical studies have shown that long-term exposure to ultraviolet light can cause light-induced diseases such as erythema, skin aging, and cataracts, and long-term exposure to ultraviolet light can also increase the risk of skin cancer. However, there is no corresponding evaluation standard for the impact of ultraviolet light penetration on the human body by semi-transparent organic photovoltaics. Therefore, establishing and evaluating the safety of semi-transparent organic photovoltaic devices is crucial for their commercial application.

[0003] Since the existing semi-transparent organic photovoltaic device structure does not take into account the light protection design of ultraviolet light, the integration of dual substrates and devices brought about by simply connecting ultraviolet filters in series will lead to a decrease in device transmittance and complicate the experimental process. Summary of the invention

[0004] In view of the deficiencies of the prior art, the present invention provides a UV-proof semi-transparent organic photovoltaic device structure and a preparation method thereof;

[0005] The present invention also provides an analysis method for the actinic ultraviolet hazard of a semi-transparent organic photovoltaic device (the hazard caused by ultraviolet light with a wavelength of 200-400nm is called actinic ultraviolet hazard).

[0006] The present invention designs an ultraviolet filter layer compatible with the experimental process based on the semi-transparent device to optimize the ultraviolet light protection of the device while reducing the impact on the transmittance of the device. The experimental conditions of the ultraviolet filter layer are mild, and damage to the underlying semi-transparent organic photovoltaic device can be avoided during the preparation process, thus achieving an effective combination of the two. The device based on the ultraviolet filter layer structure can improve the ultraviolet light protection of the device to the exemption level while maintaining the photoelectric performance and visible light transmittance of the semi-transparent photovoltaic device.

[0007] Terminology explanation:

[0008] 1. PC 71 BM: It is a polymer photovoltaic material with the molecular formula [6,6]-Phenyl-C71-butyric acidmethyl ester, mainly used as an acceptor material for organic solar cells.

[0009] 2. PM6: It is a polymer photovoltaic material with the molecular formula Poly[(2,6-(4,8-bis(5-(2-ethylhexyl-3-fluoro)thiophen-2-yl)-benzo[1,2-b:4,5-b']dithiophene))-alt-(5,5-(1',3'-di-2-thienyl-5',7'-bis(2-ethylhexyl)benzo[1',2'-c:4',5'-c']dithiophene-4,8-dione)], mainly used as a donor material for organic solar cells.

[0010] 3. PBDB-T: It is a polymer photovoltaic material with the molecular formula of Poly[(2,6-(4,8-bis(5-(2-ethylhexyl)thiophen-2-yl)-benzo[1,2-b:4,5-b']dithiophene))-alt-(5,5-(1',3'-di-2-thienyl-5',7'-bis(2-ethylhexyl)benzo[1',2'-c:4',5'-c']dithiophene-4,8-dione)], mainly used as a donor material for organic solar cells.

[0011] 4. PTB7-Th: It is a polymer photovoltaic material with the molecular formula Poly[4,8-bis(5-(2-ethylhexyl)thiophen-2-yl)benzo[1,2-b;4,5-b']dithiophene-2,6-diyl-alt-(4-(2-ethylhexyl)-3-fluorothieno[3,4-b]thiophene-)-2-carboxylate-2-6-diyl)], mainly used as a donor material for organic solar cells.

[0012] 5. D18: It is a polymer photovoltaic material with the molecular formula of Poly[(2,6-(4,8-bis(5-(2-ethylhexyl-3-fluoro)thiophen-2-yl)-benzo[1,2-b:4,5-b']dithiophene))-alt-5,5'-(5,8-bis(4-(2-butyloctyl)thiophen-2-

[0013] yl)dithieno[3',2':3,4;2”,3”:5,6]benzo[1,2-c][1,2,5]thiadiazole)], mainly used as donor material for organic solar cells.

[0014] 6. Y6: It is a polymer photovoltaic material with the molecular formula of 2,2'-((2Z,2'Z)-((12,13-bis(2-ethylhexyl)-3,9-diundecyl-12,13-dihydro-[1,2,5]thiadiazolo[3,4-e]thieno[2",3'':4',5']thieno[2',3':4,5]pyrrolo[3,2-

[0015] g]thieno[2',3':4,5]thieno[3,2-b]indole-2,10-diyl)bis(methanylylidene))bis(5,6-difluoro-3-oxo-2,3-

[0016] dihydro-1H-indene-2,1-diylidene))dimalononitrile, mainly used as acceptor material for organic solar cells.

[0017] 7. BTP-eC9: It is a polymer photovoltaic material with the molecular formula of 2,2'-[[12,13-Bis(2-butyloctyl)-12,13-dihydro-3,9-dinonylbisthieno[2”,3”:4',5']thieno[2',3':4,5]pyrrolo[3,2-e:2',3'-g][2,1,3]benzothiadiazole-2,10-diyl]bis[methylidyne(5,6-chloro-3-oxo-1H-indene-2,1(3H)-diylidene)]]bis[propanedinitrile], which is mainly used as an acceptor material for organic solar cells.

[0018] 8. ITIC: It is a polymer photovoltaic material with the molecular formula of 3,9-bis(2-methylene-(3-(1,1-dicyanomethylene)-indanone))-5,5,11,11-tetrakis(4-hexylphenyl)-dithieno[2,3-d:2',3'-d']-s-indaceno[1,2-b:5,6-

[0019] b']dithiophene, mainly used as acceptor material in organic solar cells.

[0020] 9. BTA3: It is a polymer photovoltaic material with the molecular formula of 2,2'-((5Z,5'Z)-5,5'-((7,7'-(4,4,9,9-tetrakis(4-hexylphenyl)-4,9-dihydro-s-indaceno[1,2-b:5,6-b']dithiophene-2,7-diyl)bis(2-octyl-2H-

[0021] benzo[d][1,2,3]triazole-7,4-diyl))bis(methanylylidene))bis(3-ethyl-4-oxothiazolidine-5,2-

[0022] diylidene))dimalononitrile, mainly used as acceptor material for organic solar cells.

[0023] 10. IEICO-4F: It is a polymer photovoltaic material with the molecular formula of 2,2'-((2Z,2'Z)-(((4,4,9,9-tetrakis(4-hexylphenyl)-4,9-dihydro-sindaceno[1,2-b:5,6-b']dithiophene-2,7-diyl)bis(4-((2-

[0024] ethylhexyl)oxy)thiophene-5,2-diyl))bis(methanylylidene))bis(5,6-difluoro-3-oxo-2,3-dihydro-1H-indene-2,1-diylidene))dimalononitrile is mainly used as an acceptor material for organic solar cells.

[0025] 11. N3: It is a polymer photovoltaic material with the molecular formula of 2,2'–((2Z,2'Z)–((12,13–bis(3–ethylheptyl)–3,9–diundecyl–12,13–dihydro–[1,2,5]thiadiazolo[3,4–e]thieno[2”,3”:4’,5’]thieno[2’,3’:4,5]pyrrolo[3,2–g]thieno[2’,3’:4,5]thieno[3,2–b]indole–2,10–diyl)bis(methanylylidene))bis(5,6–difluoro–3–oxo–2,3–dihydro–1H–indene–2,1–diylidene))dimalononitrile. It is mainly used as an acceptor material for organic solar cells.

[0026] 12. N2200: It is a polymer photovoltaic material with the molecular formula Poly{[N,N'-bis(2-octyldodecyl)naphthalene-1,4,5,8-bis(dicarboximide)-2,6-diyl]-alt-5,5'-(2,2'-bithiophene)}, mainly used as an acceptor material for organic solar cells.

[0027] 13. L8-BO: It is a polymer photovoltaic material with the molecular formula of 2,2'-((2Z,2'Z)-((12,13-bis(2-ethylhexyl)-3,9-(2-butyloctyl)-12,13-dihydro-[1,2,5]thiadiazolo[3,4-e]thieno[2",3'':4',5']thieno[2',3':4,5]pyrrolo[3,2-g]thieno[2',3':4,5]thieno[3,2-b]indole-2,10-diyl)bis(methanylylidene))bis(5,6-difluoro-3-oxo-2,3-dihydro-1H-indene-2,1-diylidene))dimalononitrile. It is mainly used as a donor material for organic solar cells.

[0028] 14. PEDOT:PSS: PEDOT:PSS is a polymer photovoltaic material with the molecular formula Poly(3,4-ethylenedioxythiophene):Poly(styrene sulfonate). It is mainly used as a hole transport layer material for organic solar cells.

[0029] 15. PDIN: It is a polymer photovoltaic material with the molecular formula N,N'-Bis[3-(dimethylamino)propyl]perylene-3,4,9,10-tetracarboxylic diimide. It is mainly used as an electron transport layer material for organic solar cells.

[0030] The technical solution of the present invention is:

[0031] A UV-proof semi-transparent organic photovoltaic device structure comprises a substrate, an anode, a hole transport layer, an active layer, an electron transport layer, a cathode and a UV filter layer which are grown in sequence from bottom to top.

[0032] Preferably, according to the present invention, the UV filter layer is prepared by the following method, comprising:

[0033] The UV filter layer is prepared by alternately evaporating LiF and TeO2, and its function is to filter ultraviolet light with a wavelength below 380nm.

[0034] Further preferably, in one LiF and TeO2 alternating evaporation cycle,

[0035] In less than 5х10 -4 Pa vacuum conditions, LiF was prepared by thermal evaporation, with a growth rate of

[0036] In less than 5х10 -4 Pa vacuum conditions, TeO2 was prepared by thermal evaporation, with a growth rate of

[0037] Since the preparation conditions of LiF and TeO2 are mild, the preparation process will not affect the semi-transparent organic photovoltaic device, thus realizing the integrated process of UV filter layer structure and semi-transparent organic photovoltaic device.

[0038] According to the preferred embodiment of the present invention, the active layer is PM6:Y6, PM6:L8-BO, PM6:BTP-eC9, D18:L8-BO, D18:N3, PBDB-T:ITIC, PBDB-T:N2200, PBDB-T:BTA3, PTB7-Th:IEICO-4F, PTB7-Th:PC 71 BM, P3HT:PC71 BM Any of the eleven binary material systems.

[0039] Preferably, according to the present invention, the mass ratio of PM6 to Y6 in PM6:Y6 is 1:1.2; the mass ratio of PM6 to BTP-eC9 in PM6:BTP-eC9 is 1:1.2; the mass ratio of PM6 to L8-BO in PM6:L8-BO is 1:1.2; the mass ratio of D18 to L8-BO in D18:L8-BO is 1:1.2; the mass ratio of D18 to N3 in D18:N3 is 0.7:1.6; the mass ratio of PBDB-T to ITIC in PBDB-T:ITIC is 1:1; the mass ratio of PBDB-T to N2200 in PBDB-T:N2200 is 2:1; the mass ratio of PBDB-T to BTA3 in PBDB-T:BTA3 is 1:1; the mass ratio of PTB7-Th to IEICO-4F in PTB7-Th:IEICO-4F is 1:1.5; PTB7-Th:PC 71 PTB7-Th and PC in BM 71 The mass ratio of BM is 1:1.5; P3HT:PC 71 P3HT and PC in BM 71 The mass ratio of BM is 1:1.

[0040] Preferably according to the present invention, the substrate is a glass substrate, the anode is a transparent conductive film, the material of the hole transport layer is PEDOT:PSS, the material of the electron transport layer is PDIN, and the cathode is an ultra-thin metal silver electrode.

[0041] The method for preparing the above-mentioned ultraviolet light-proof semi-transparent organic photovoltaic device structure comprises:

[0042] Spin coating the hole transport layer on the substrate surface;

[0043] In a nitrogen atmosphere, spin coating an active layer material on the hole transport layer to prepare an active layer;

[0044] Spin coating the electron transport layer on the surface of the active layer;

[0045] Under vacuum conditions, a cathode is prepared on the electron transport layer;

[0046] The UV filter layer is evaporated on the cathode to obtain the result.

[0047] Preferably, according to the present invention, a UV filter layer is evaporated on the cathode; comprising:

[0048] A UV filter layer is further evaporated on the cathode. The filter layer structure is an ABA structure with more than 8 periods, A is LiF with a thickness of 20 nm, and B is TeO2 with a thickness of 62 nm.

[0049] Preferably, according to the present invention, in a nitrogen atmosphere, the active layer is prepared by spin coating the active layer material on the hole transport layer; comprising:

[0050] In a nitrogen atmosphere, an active layer material is spin-coated on the hole transport layer, the active layer thickness is 70-120 nm, and annealing is performed at 100-120° C. for 10-15 min.

[0051] According to the preferred embodiment of the present invention, the substrate is ITO conductive glass; before preparing the hole transport layer, the following operations are performed:

[0052] The ITO conductive glass was ultrasonically cleaned with a cleaning agent, deionized water, acetone, anhydrous ethanol and isopropanol in sequence, dried with nitrogen, and then treated with UV for 10-15 minutes.

[0053] Preferably, according to the present invention, a hole transport layer is prepared by spin coating on the surface of a substrate; comprising:

[0054] Spin coat PEDOT:PSS on the conductive glass surface and anneal at 120-150℃ for 10-15min.

[0055] Preferably, according to the present invention, the electron transport layer is prepared by spin coating on the surface of the active layer; comprising:

[0056] 2 mg / mL PDIN solution was spin-coated onto the active layer at a speed of 3000-5000 rpm for 20-40 s.

[0057] Preferably, according to the present invention, a cathode is prepared on an electron transport layer under vacuum conditions; comprising:

[0058] In less than 5х10 -4 A 12 nm Ag electrode was prepared by thermal evaporation under vacuum conditions of 0.03 Pa.

[0059] The beneficial effects of the present invention are:

[0060] The present invention further evaporates a UV filter layer on the metal cathode to block the transmission of ultraviolet light without affecting the visible light transmittance and battery performance. The filter layer is integrated on the solar cell structure by evaporation, and can effectively reflect ultraviolet light with a wavelength below 380nm without losing device performance. Thanks to the absorption of ultraviolet light by the UV filter layer, the threat of ultraviolet light to the human body is reduced when the device is running, providing guidance for the prevention of photobiological safety in large-scale commercial applications of semi-transparent organic photovoltaics. BRIEF DESCRIPTION OF THE DRAWINGS

[0061] Figure 1 A schematic diagram of the structure of the ultraviolet light-proof semi-transparent organic photovoltaic device of the present invention;

[0062] Figure 2 It is the actinic ultraviolet hazard diagram corresponding to 11 groups of material systems;

[0063] Figure 3 Schematic diagram comparing the exposure time of the semi-transparent organic photovoltaic active layer film with and without the addition of a UV filter layer. DETAILED DESCRIPTION

[0064] The present invention will be further defined below in conjunction with the accompanying drawings and embodiments, but is not limited thereto.

[0065] Example 1

[0066] A UV-proof semi-transparent organic photovoltaic device structure, such as Figure 1 As shown, it includes a substrate, an anode, a hole transport layer, an active layer, an electron transport layer, a cathode and a UV filter layer grown in sequence from bottom to top.

[0067] Example 2

[0068] The difference of the anti-ultraviolet light semi-transparent organic photovoltaic device structure according to Example 1 is that:

[0069] The UV filter layer is prepared by the following method, comprising:

[0070] The UV filter layer is prepared by alternately evaporating LiF and TeO2, and its function is to filter ultraviolet light with a wavelength below 380nm.

[0071] In a LiF and TeO2 alternating evaporation cycle, the -4 Pa vacuum conditions, LiF was prepared by thermal evaporation, with a growth rate of In less than 5х10 -4 Pa vacuum conditions, TeO2 was prepared by thermal evaporation, with a growth rate of

[0072] Since the preparation conditions of LiF and TeO2 are mild, the preparation process will not affect the semi-transparent organic photovoltaic device, thus realizing the integrated process of UV filter layer structure and semi-transparent organic photovoltaic device.

[0073] Active layer: PM6:Y6, PM6:L8-BO, PM6:BTP-eC9, D18:L8-BO, D18:N3, PBDB-T:ITIC, PBDB-T:N2200, PBDB-T:BTA3, PTB7-Th:IEICO-4F, PTB7-Th:PC 71 BM, P3HT:PC 71 BM Any of the eleven binary material systems.

[0074] The mass ratio of PM6 to Y6 in PM6:Y6 is 1:1.2; the mass ratio of PM6 to BTP-eC9 in PM6:BTP-eC9 is 1:1.2; the mass ratio of PM6 to L8-BO in PM6:L8-BO is 1:1.2; the mass ratio of D18 to L8-BO in D18:L8-BO is 1:1.2; the mass ratio of D18 to N3 in D18:N3 is 0.7:1.6; the mass ratio of PBDB-T to ITIC in PBDB-T:ITIC is 1:1; the mass ratio of PBDB-T to N2200 in PBDB-T:N2200 is 2:1; the mass ratio of PBDB-T to BTA3 in PBDB-T:BTA3 is 1:1; the mass ratio of PTB7-Th to IEICO-4F in PTB7-Th:IEICO-4F is 1:1.5; PTB7-Th:PC 71 PTB7-Th and PC in BM 71 The mass ratio of BM is 1:1.5; P3HT:PC 71 P3HT and PC in BM 71 The mass ratio of BM is 1:1.

[0075] The substrate is a glass substrate, the anode is a transparent conductive film, the material of the hole transport layer is PEDOT:PSS, the material of the electron transport layer is PDIN, and the cathode is an ultra-thin metal silver electrode.

[0076] This embodiment designs a 380nm long-wave filter layer integrated into a semi-transparent organic photovoltaic device. The degree of ultraviolet hazard of different devices is measured by the actinic ultraviolet hazard dose. Considering that the main difference between different semi-transparent organic devices lies in the active layer, the change of the actinic ultraviolet hazard dose corresponding to the active layer is mainly analyzed.

[0077] Actinic UV Hazard Dose E s Evaluation method: Test the transmission spectrum of the active layer heterojunction to obtain the AM1.5G solar spectrum power distribution function after the device is activated, and calculate E by the following formula: s :

[0078]

[0079] In the formula, E λ (λ) is the spectral power distribution function of the transmitted light source, S UV (λ) is the actinic UV hazard weighting function, and Δλ is the wavelength interval (in nm).

[0080] Get the actinic ultraviolet hazard dose E of all devices s After that, you can use E s Then the safe exposure time t corresponding to different active layers is calculateds When the human body is exposed to sunlight for longer than this value, the risk of illness will increase significantly.

[0081] Actinic UV Hazard Exposure Time t s The calculation method is:

[0082]

[0083] Where, 30 J·m -2 The limit for effective radiation exposure to UV light.

[0084] The protective effects of different semi-transparent organic photovoltaic and UV filter layers against photochemical ultraviolet hazards are shown as follows: Figure 2 As shown in Table 1. As can be seen from the figure, PTB7-Th:PC 71 BM has the best protection effect against actinic UV damage among the 11 semi-transparent photovoltaic materials, and the final residual dose of actinic UV damage is only half of that of other materials. The UV filter layer shows the best protection against actinic UV damage, and the final residual dose of actinic UV damage is only 3% of that of other materials. The exposure time of different semi-transparent organic photovoltaics and UV filter layers to actinic UV damage is as follows Figure 3 The average exposure time obtained when the active layer material is used alone is about 2000s. The best PTB7-Th:PC 71 The exposure time of BM film is 4578s, which cannot meet the demand of long-term operation of semi-transparent photovoltaic in real life. After the UV filter layer is applied, the exposure time reaches 30000s, reaching the exemption level, eliminating the threat of photochemical ultraviolet hazards to human body.

[0085] Table 1

[0086]

[0087]

[0088] Example 3

[0089] The method for preparing the ultraviolet light-proof semi-transparent organic photovoltaic device structure described in Embodiment 1 or 2 comprises:

[0090] Spin coating the hole transport layer on the substrate surface;

[0091] In a nitrogen atmosphere, spin coating an active layer material on the hole transport layer to prepare an active layer;

[0092] Spin coating the electron transport layer on the surface of the active layer;

[0093] Under vacuum conditions, a cathode is prepared on the electron transport layer;

[0094] The UV filter layer is evaporated on the cathode to obtain the result.

[0095] Example 4

[0096] The method for preparing the anti-ultraviolet light semi-transparent organic photovoltaic device structure according to Example 3 is different in that:

[0097] A UV filter layer is deposited on the cathode; comprising:

[0098] A UV filter layer is further evaporated on the cathode. The filter layer structure is an ABA structure with more than 8 periods, A is LiF with a thickness of 20 nm, and B is TeO2 with a thickness of 62 nm.

[0099] In a nitrogen atmosphere, spin coating an active layer material on the hole transport layer to prepare an active layer; comprising:

[0100] In a nitrogen atmosphere, the active layer material was spin-coated on the hole transport layer at a rotation speed of 3000 rpm for 50 s, with an active layer thickness of 70-120 nm, and annealed at 100° C. for 10 min.

[0101] The substrate is ITO conductive glass; before preparing the hole transport layer, perform the following operations:

[0102] The ITO conductive glass was ultrasonically cleaned with a cleaning agent, deionized water, acetone, anhydrous ethanol and isopropanol in sequence, dried with nitrogen, and then treated with UV for 15 minutes.

[0103] Spin coating to prepare a hole transport layer on a substrate surface; comprising:

[0104] Spin coat PEDOT:PSS on the conductive glass surface and anneal at 150℃ for 10-15min.

[0105] The electron transport layer is prepared by spin coating on the surface of the active layer; comprising:

[0106] 2 mg / mL PDIN solution was spin coated onto the active layer at a speed of 5000 rpm for 30 s. A cathode was prepared on the electron transport layer under vacuum conditions; including:

[0107] In 4х10 -4 A 12 nm Al electrode was prepared by thermal evaporation under vacuum conditions of 1.3 Pa.

Claims

1. A UV-proof semi-transparent organic photovoltaic device structure, It is characterized in that The invention comprises a substrate, an anode, a hole transport layer, an active layer, an electron transport layer, a cathode and a UV filter layer which are grown in sequence from bottom to top.

2. The anti-ultraviolet light semi-transparent organic photovoltaic device structure according to claim 1, It is characterized in that The UV filter layer is prepared by the following method, comprising: LiF and TeO 2 The UV filter layer is prepared by alternate evaporation.

3. The anti-ultraviolet light semi-transparent organic photovoltaic device structure according to claim 2, It is characterized in that In a LiF and TeO 2 During the alternating evaporation cycle, the -4 Pa vacuum conditions, LiF was prepared by thermal evaporation, with a growth rate of In less than 5х10 -4 TeO was prepared by thermal evaporation under vacuum conditions of 1.3 Pa. 2 , the growth rate is 4. The anti-ultraviolet light semi-transparent organic photovoltaic device structure according to claim 1, It is characterized in that The active layer is PM6:Y6, PM6:L8-BO, PM6:BTP-eC9, D18:L8-BO, D18:N3, PBDB-T:ITIC, PBDB-T:N2200, PBDB-T:BTA3, PTB7-Th:IEICO-4F, PTB7-Th:PC 71 BM, P3HT:PC 71 BM Any of the eleven binary material systems.

5. The anti-ultraviolet light semi-transparent organic photovoltaic device structure according to claim 4, It is characterized in that The mass ratio of PM6 to Y6 in PM6:Y6 is 1:1.2; the mass ratio of PM6 to BTP-eC9 in PM6:BTP-eC9 is 1:1.2; the mass ratio of PM6 to L8-BO in PM6:L8-BO is 1:1.2; the mass ratio of D18 to L8-BO in D18:L8-BO is 1:1.2; the mass ratio of D18 to N3 in D18:N3 is 0.7:1.6; the mass ratio of PBDB-T to ITIC in PBDB-T:ITIC is 1:1; the mass ratio of PBDB-T to N2200 in PBDB-T:N2200 is 2:1; the mass ratio of PBDB-T to BTA3 in PBDB-T:BTA3 is 1:1; the mass ratio of PTB7-Th to IEICO-4F in PTB7-Th:IEICO-4F is 1:1.5; PTB7-Th:PC 71 PTB7-Th and PC in BM 71 The mass ratio of BM is 1:1.5; P3HT:PC 71 P3HT and PC in BM 71 The mass ratio of BM is 1:

1.

6. The anti-ultraviolet light semi-transparent organic photovoltaic device structure according to claim 1, It is characterized in that The substrate is a glass substrate, the anode is a transparent conductive film, the hole transport layer is made of PEDOT:PSS, the electron transport layer is made of PDIN, and the cathode is an ultra-thin metal silver electrode.

7. A method for preparing a UV-proof semi-transparent organic photovoltaic device structure according to any one of claims 1 to 6, It is characterized in that include: Spin coating the hole transport layer on the substrate surface; In a nitrogen atmosphere, spin coating an active layer material on the hole transport layer to prepare an active layer; Spin coating the electron transport layer on the surface of the active layer; Under vacuum conditions, a cathode is prepared on the electron transport layer; The UV filter layer is evaporated on the cathode to obtain the result.

8. The method for preparing the ultraviolet light-proof semi-transparent organic photovoltaic device structure according to claim 7, It is characterized in that A UV filter layer is deposited on the cathode; comprising: A UV filter layer is further evaporated on the cathode. The filter layer structure is an ABA structure with more than 8 periods, A is LiF with a thickness of 20 nm, and B is TeO 2 , thickness 62nm; Further preferably, in a nitrogen atmosphere, the active layer is prepared by spin coating an active layer material on the hole transport layer; comprising: In a nitrogen atmosphere, an active layer material is spin-coated on the hole transport layer, the active layer thickness is 70-120 nm, and annealing is performed at 100-120° C. for 10-15 min.

9. The method for preparing the ultraviolet light-proof semi-transparent organic photovoltaic device structure according to claim 7, It is characterized in that The substrate is ITO conductive glass; before preparing the hole transport layer, the following operations are performed: The ITO conductive glass was ultrasonically cleaned with a cleaning agent, deionized water, acetone, anhydrous ethanol and isopropanol in sequence, dried with nitrogen, and then treated with UV for 10-15 minutes; Further preferably, the hole transport layer is prepared by spin coating on the surface of the substrate; comprising: Spin coat PEDOT:PSS on the conductive glass surface and anneal at 120-150℃ for 10-15min.

10. The method for preparing the ultraviolet light-proof semi-transparent organic photovoltaic device structure according to any one of claims 7 to 9, It is characterized in that The electron transport layer is prepared by spin coating on the surface of the active layer; comprising: Spin coat 2 mg / mL PDIN solution onto the active layer at a speed of 3000-5000 rpm for 20-40 s; Further preferably, under vacuum conditions, a cathode is prepared on the electron transport layer; comprising: In less than 5х10 -4 A 12 nm Ag electrode was prepared by thermal evaporation under vacuum conditions of 0.03 Pa.