Nail polish gel base material based on visible light curing and preparation method thereof

By using specific proportions of oligomers and photoinitiators in the nail polish glue, the nail polish glue base that can be cured under visible and ultraviolet light is achieved, and the skin damage and adhesion caused by ultraviolet light curing is solved. Poor problems improve flexibility and curing efficiency.

CN119033629APending Publication Date: 2024-11-29GUANGDONG INNOVATION SCIENCE & TECHNOLOGY APPLICATION CO LTD

Patent Information

Application Number
CN202411164734.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing nail polish glues are cured using ultraviolet light, which leads to skin damage and poor adhesion.

Method used

Using a nail polish glue base material based on visible light curing, it is prepared by specific proportions of oligomers, photoinitiators, monomer solvents, leveling agents and defoaming agents to cure under visible light and ultraviolet light, reducing ultraviolet light Damage to the skin and improve flexibility and adhesion.

Benefits of technology

Shorten curing time, reduces the damage to the skin by UV rays, improves the flexibility and adhesion of nail polish glue, ensuring a longer lasting shine and a more convenient coating process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention belongs to the technical field of chemical materials, and particularly discloses a nail polish gel base material based on visible light curing and a preparation method of the nail polish gel base material. The nail polish gel base material comprises 60-80 parts of an oligomer, 3-5 parts of a photoinitiator, 15-30 parts of a monomer solvent, 0.5-2 parts of a leveling agent and 0.5-2 parts of a defoaming agent. Wherein the oligomer is selected from three oligomers of polyester acrylate, polyurethane acrylic resin and epoxy acrylic resin which are mixed according to a reasonable proportion, and the prepared nail polish gel base material is moderate in viscosity, convenient to coat, good in flexibility and strong in adhesive force; wherein the photoinitiator 784, the photoinitiator 819 and the photoinitiator 184 are compounded according to a certain proportion and have a synergistic effect, so that the curing efficiency is improved, the curing time is greatly shortened, the curing can be completed only in 20-40 seconds, the waiting time of customers is shortened, and the curing can be completed under visible light; and the injury of ultraviolet irradiation to the hand skin of an operator and a customer is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The invention belongs to the technical field of chemical materials, and in particular relates to a nail polish base material based on visible light curing and a preparation method thereof. [Background technology]

[0002] Nail polish, also known as nail glue, has been widely used in the nail industry in recent years. Compared with general nail polish, nail polish itself has its own characteristics, such as biochemical nail polish, which is environmentally friendly, non-toxic, healthy and safe. In addition, it has the common advantages of both glue and nail polish, with rich and clear color, easy application, and longer-lasting gloss. Therefore, nail polish has gradually replaced nail polish.

[0003] At present, most of the nail polish glue used in the market adopts ultraviolet light curing to speed up the drying of nail polish, reduce waiting time, and avoid accidental damage to the shape during the drying process. However, after long-term use, ultraviolet light curing is easy to cause damage to the skin of the hands of operators and customers who do manicures, causing their skin to darken and increasing the risk of cancer. In addition, the existing nail polish glue has poor flexibility and adhesion, and is easy to break and fall off. [Summary of the invention]

[0004] In view of the defects of the prior art, the purpose of the present invention is to provide a nail polish base material based on visible light curing and a preparation method thereof, so as to achieve curing under both visible light and ultraviolet light and reduce the damage of ultraviolet light to the skin.

[0005] In order to achieve the above technical effects, the first aspect of the present invention is to provide a visible light-cured nail polish base material, which includes the following components by mass: 60-80 parts of oligomer, 3-5 parts of photoinitiator, 15-30 parts of monomer solvent, 0.5-2 parts of leveling agent, and 0.5-2 parts of defoaming agent.

[0006] Preferably, the oligomer is composed of polyester acrylate, polyurethane acrylate and epoxy acrylate, and the mass ratio of each component is polyester acrylate: polyurethane acrylate: epoxy acrylate = (5-20): (20-50): (5-10). The three are compounded and used within this ratio range, the viscosity is moderate, and it is easy to mix and apply. The prepared nail polish base material has good flexibility and strong adhesion.

[0007] Preferably, the mass ratio of each component in the oligomer is polyester acrylate: polyurethane acrylate: epoxy acrylate = (15-20): (40-50): (5-10), and more preferably, polyester acrylate: polyurethane acrylate: epoxy acrylate = 15:40:10.

[0008] Preferably, the photoinitiator includes photoinitiator 784, photoinitiator 184 and photoinitiator 819. These photoinitiators have certain absorption peaks in the ultraviolet and visible light bands. By compounding the photoinitiator, it can not only maintain ultraviolet absorption to initiate resin polymerization, but also absorb light energy at a specific visible light wavelength to play an initiating role. Photoinitiator 784 has the function of a co-initiator. It can absorb visible light to generate free radicals, and rapidly proliferate free radicals, triggering other photoinitiators to react quickly and shorten the curing time.

[0009] Preferably, the mass ratio of each initiator in the photoinitiator is photoinitiator 784: photoinitiator 184: photoinitiator 819 = (0.5-1.5): (0.2-1): (1-3). When the three are compounded and used within this range, the three can enhance synergy and have high curing efficiency.

[0010] Preferably, the mass ratio of each initiator in the photoinitiator is photoinitiator 784:photoinitiator 184:photoinitiator 819=(1-1.5):(0.5-1):(2-3); more preferably, photoinitiator 784:photoinitiator 184:photoinitiator 819=1.5:0.5:2.

[0011] Preferably, the monomer solvent is selected from one or more of hydroxyethyl methacrylate (HEMA), hydroxypropyl methacrylate (HPMA), butyl acrylate (BA) and the like.

[0012] Preferably, the leveling agent can be selected from commonly used leveling agents in the art, and specifically can be selected from one or more of BYK-UV3510, BYK-341, BYK-344, BYK-345, BYK-346, BYK-347, and BYK-348.

[0013] Preferably, the defoaming agent can be selected from the defoaming agents commonly used in the art, and can be specifically selected from one of polysiloxane defoaming agents and polyether defoaming agents.

[0014] The second aspect of the present invention is to provide a method for preparing the above-mentioned nail polish base material, comprising the following steps:

[0015] (1) Weighing a certain amount of polyester acrylate, polyurethane acrylate and epoxy acrylate according to the formula ratio, placing them in a stirring tank and mixing them evenly, adding a portion of the monomer solvent and stirring until the oligomer is completely dissolved;

[0016] (2) Weigh a certain amount of photoinitiator 784, photoinitiator 184 and photoinitiator 819 according to the formula ratio, place them in a stirring tank, add a portion of the monomer solvent, and stir until the photoinitiator is completely dissolved;

[0017] (3) adding the oligomer dissolved in step (1) to the photoinitiator dissolved in step (2), and stirring at 50 to 60° C.;

[0018] (4) adding a leveling agent and a defoaming agent to the mixture prepared in step (3), and stirring until completely dissolved;

[0019] (5) After filtering with a sieve, defoam in a vacuum drying oven, test the viscosity, and discharge the material.

[0020] Preferably, in step (1), the mass ratio of the monomer solvent used to dissolve the oligomer to the oligomer is (1-2.5):(6-8).

[0021] Preferably, in step (2), the mass ratio of the monomer solvent used to dissolve the photoinitiator to the photoinitiator is 5:(3-5).

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The nail polish base material of the present invention is prepared by mixing three oligomers of polyester acrylate, polyurethane acrylic resin and epoxy acrylic resin in a reasonable proportion. The prepared oligomer has moderate viscosity and is easy to apply. The nail polish base material prepared by the oligomer has good flexibility and strong adhesion.

[0024] The nail polish base material of the present invention uses a photoinitiator with an absorption peak under visible light, so that it can be cured under visible light, reducing the damage caused by ultraviolet radiation to the operator and the customer's hand skin;

[0025] The photoinitiator in the nail polish base material of the present invention is selected from photoinitiator 784, photoinitiator 819, and photoinitiator 184, which are compounded in a certain ratio. The three are synergistic, improve the curing efficiency, and greatly shorten the curing time. The curing can be completed in only 20 to 40 seconds, which reduces the waiting time for customers.

[0026] When preparing the nail polish base material of the present invention, the oligomer and the photoinitiator are dissolved separately by a monomer solvent and then mixed, so as to ensure that the substances are mixed evenly and react thoroughly. [Specific implementation method]

[0027] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is described by the following specific embodiments, but is by no means limited thereto. The following are preferred embodiments of the present invention, which are only used to describe the present invention and cannot be understood as limiting the present invention. It should be pointed out that any modification, equivalent substitution and improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

[0028] The monomer solvent described in the following examples is selected from one of hydroxyethyl methacrylate (HEMA), hydroxypropyl methacrylate (HPMA), butyl acrylate (BA) and the like.

[0029] The leveling agent is selected from one of BYK-UV3510, BYK-341, BYK-344, BYK-345, BYK-346, BYK-347 and BYK-348.

[0030] The defoamer is selected from one of polysiloxane defoamer and polyether defoamer.

[0031] The parts described in the following examples are all parts by mass.

[0032] Example 1

[0033] (1) Weigh 15 parts of polyester acrylate, 40 parts of polyurethane acrylate and 10 parts of epoxy acrylate respectively, place them in a stirring tank and mix them evenly, add 20 parts of monomer solvent (HEMA) and stir until the oligomer is completely dissolved;

[0034] (2) Weigh 1.5 parts of photoinitiator 784, 0.5 parts of photoinitiator 184, and 2 parts of photoinitiator 819 respectively and place them in a stirring tank, add 5 parts of monomer solvent (HEMA), and stir until the photoinitiators are completely dissolved;

[0035] (3) adding the oligomer dissolved in step (1) to the photoinitiator dissolved in step (2), and stirring at 50° C. for 30 minutes;

[0036] (4) adding 0.5 parts of leveling agent (BYK-UV3510) and 0.5 parts of defoamer (polysiloxane defoamer) to the mixture prepared in step (3), and stirring until completely dissolved;

[0037] (5) After filtering with a sieve, defoam in a vacuum drying oven, test the viscosity, and discharge the material.

[0038] Example 2

[0039] (1) Weigh 20 parts of polyester acrylate, 50 parts of polyurethane acrylate and 5 parts of epoxy acrylate respectively, place them in a stirring tank and mix them evenly, add 25 parts of monomer solvent (HEMA) and stir until the oligomer is completely dissolved;

[0040] (2) Weigh 1 part of photoinitiator 784, 1 part of photoinitiator 184, and 2 parts of photoinitiator 819 respectively and place them in a stirring tank, add 5 parts of monomer solvent (HEMA), and stir until the photoinitiators are completely dissolved;

[0041] (3) adding the oligomer dissolved in step (1) to the photoinitiator dissolved in step (2), and stirring at 50° C. for 30 minutes;

[0042] (4) adding 0.8 parts of leveling agent (BYK-345) and 0.5 parts of defoamer (polysiloxane defoamer) to the mixture prepared in step (3), and stirring until completely dissolved;

[0043] (5) After filtering with a sieve, defoam in a vacuum drying oven, test the viscosity, and discharge the material.

[0044] Example 3

[0045] (1) Weigh 5 parts of polyester acrylate, 50 parts of polyurethane acrylate and 5 parts of epoxy acrylate respectively, put them into a stirring tank and mix them evenly, add 10 parts of monomer solvent (HPMA) and stir until the oligomer is completely dissolved;

[0046] (2) Weigh 0.5 parts of photoinitiator 784, 0.5 parts of photoinitiator 184, and 2.5 parts of photoinitiator 819 respectively and place them in a stirring tank, add 5 parts of monomer solvent (HPMA), and stir until the photoinitiators are completely dissolved;

[0047] (3) adding the oligomer dissolved in step (1) to the photoinitiator dissolved in step (2), and stirring at 55° C. for 30 minutes;

[0048] (4) adding 1 part of leveling agent (BYK-347) and 1 part of defoamer (polyether defoamer) to the mixture prepared in step (3), and stirring until completely dissolved;

[0049] (5) After filtering with a sieve, defoam in a vacuum drying oven, test the viscosity, and discharge the material.

[0050] Example 4

[0051] (1) Weigh 17 parts of polyester acrylate, 45 parts of polyurethane acrylate and 8 parts of epoxy acrylate respectively, place them in a stirring tank and mix them evenly, add 15 parts of monomer solvent (HPMA) and stir until the oligomer is completely dissolved;

[0052] (2) Weigh 1 part of photoinitiator 784, 0.5 parts of photoinitiator 184, and 3 parts of photoinitiator 819 respectively and place them in a stirring tank, add 5 parts of monomer solvent (HPMA), and stir until the photoinitiators are completely dissolved;

[0053] (3) adding the oligomer dissolved in step (1) to the photoinitiator dissolved in step (2), and stirring at 50° C. for 30 minutes;

[0054] (4) adding 1.5 parts of a leveling agent (BYK-347) and 1 part of a defoamer (polyether defoamer) to the mixture prepared in step (3), and stirring until completely dissolved;

[0055] (5) After filtering with a sieve, defoam in a vacuum drying oven, test the viscosity, and discharge the material.

[0056] Example 5

[0057] (1) Weigh 20 parts of polyester acrylate, 50 parts of polyurethane acrylate and 10 parts of epoxy acrylate respectively, place them in a stirring tank and mix them evenly, add 25 parts of monomer solvent (BA) and stir until the oligomer is completely dissolved;

[0058] (2) Weigh 1.5 parts of photoinitiator 784, 0.5 parts of photoinitiator 184, and 1 part of photoinitiator 819 respectively and place them in a stirring tank, add 5 parts of monomer solvent (BA), and stir until the photoinitiators are completely dissolved;

[0059] (3) adding the oligomer dissolved in step (1) to the photoinitiator dissolved in step (2), and stirring at 55° C. for 30 minutes;

[0060] (4) adding 1 part of leveling agent (BYK-341) and 2 parts of defoamer (polysiloxane defoamer) to the mixture prepared in step (3), and stirring until completely dissolved;

[0061] (5) After filtering with a sieve, defoam in a vacuum drying oven, test the viscosity, and discharge the material.

[0062] Example 6

[0063] (1) Weigh 20 parts of polyester acrylate, 30 parts of polyurethane acrylate and 10 parts of epoxy acrylate respectively, place them in a stirring tank and mix them evenly, add 25 parts of monomer solvent (BA) and stir until the oligomer is completely dissolved;

[0064] (2) Weigh 1.8 parts of photoinitiator 784, 0.2 parts of photoinitiator 184, and 3 parts of photoinitiator 819 respectively and place them in a stirring tank, add 5 parts of monomer solvent (BA), and stir until the photoinitiator is completely dissolved;

[0065] (3) adding the oligomer dissolved in step (1) to the photoinitiator dissolved in step (2), and stirring at 60° C. for 30 minutes;

[0066] (4) adding 1 part of leveling agent (BYK-341) and 2 parts of defoamer (polysiloxane defoamer) to the mixture prepared in step (3), and stirring until completely dissolved;

[0067] (5) After filtering with a sieve, defoam in a vacuum drying oven, test the viscosity, and discharge the material.

[0068] Comparative Example 1

[0069] (1) Weigh 20 parts of polyester acrylate and 45 parts of polyurethane acrylate respectively, place them in a stirring tank and mix them evenly, add 20 parts of monomer solvent (HEMA) and stir until the oligomer is completely dissolved;

[0070] (2) Weigh 1.5 parts of photoinitiator 784, 0.5 parts of photoinitiator 184, and 2 parts of photoinitiator 819 respectively and place them in a stirring tank, add 5 parts of monomer solvent (HEMA), and stir until the photoinitiators are completely dissolved;

[0071] (3) adding the oligomer dissolved in step (1) to the photoinitiator dissolved in step (2), and stirring at 50° C. for 30 minutes;

[0072] (4) adding 0.5 parts of leveling agent (BYK-UV3510) and 0.5 parts of defoamer (polysiloxane defoamer) to the mixture prepared in step (3), and stirring until completely dissolved;

[0073] (5) After filtering with a sieve, defoam in a vacuum drying oven, test the viscosity, and discharge the material.

[0074] Comparative Example 2

[0075] (1) Weigh 15 parts of polyester acrylate, 40 parts of polyurethane acrylate and 10 parts of epoxy acrylate respectively, place them in a stirring tank and mix them evenly, add 20 parts of monomer solvent (HEMA) and stir until the oligomer is completely dissolved;

[0076] (2) Weigh 1.5 parts of photoinitiator 784 and 0.5 parts of photoinitiator 184 respectively and place them in a stirring tank, add 5 parts of monomer solvent (HEMA), and stir until the photoinitiator is completely dissolved;

[0077] (3) adding the oligomer dissolved in step (1) to the photoinitiator dissolved in step (2), and stirring at 50° C. for 30 minutes;

[0078] (4) adding 0.5 parts of leveling agent BYK-UV3510) and 0.5 parts of defoamer (polysiloxane defoamer) to the mixture prepared in step (3), and stirring until completely dissolved;

[0079] (5) After filtering with a sieve, defoam in a vacuum drying oven, test the viscosity, and discharge the material.

[0080] Comparative Example 3

[0081] (1) Weigh 60 parts of polyurethane acrylate and 10 parts of epoxy acrylate respectively, place them in a stirring tank and mix them evenly, add 20 parts of monomer solvent (HEMA) and stir until the oligomer is completely dissolved;

[0082] (2) Weigh 1.5 parts of photoinitiator 784, 0.5 parts of photoinitiator 184, and 2 parts of photoinitiator 819 respectively and place them in a stirring tank, add 5 parts of monomer solvent (HEMA), and stir until the photoinitiators are completely dissolved;

[0083] (3) adding the oligomer dissolved in step (1) to the photoinitiator dissolved in step (2), and stirring at 50° C. for 30 minutes;

[0084] (4) adding 0.5 parts of leveling agent (BYK-UV3510) and 0.5 parts of defoamer (polysiloxane defoamer) to the mixture prepared in step (3), and stirring until completely dissolved;

[0085] (5) After filtering with a sieve, defoam in a vacuum drying oven, test the viscosity, and discharge the material.

[0086] Comparative Example 4

[0087] (1) Weigh 75 parts of polyurethane acrylate and place them in a stirring tank and mix them evenly, then add 20 parts of monomer solvent (HEMA) and stir until the oligomer is completely dissolved;

[0088] (2) Weigh 4 parts of photoinitiator 819 and place it in a stirring tank, add 5 parts of monomer solvent (HEMA), and stir until the photoinitiator is completely dissolved;

[0089] (3) adding the oligomer dissolved in step (1) to the photoinitiator dissolved in step (2), and stirring at 50° C. for 30 minutes;

[0090] (4) adding 0.5 parts of leveling agent (BYK-UV3510) and 0.5 parts of defoamer (polysiloxane defoamer) to the mixture prepared in step (3), and stirring until completely dissolved;

[0091] (5) After filtering with a sieve, defoam in a vacuum drying oven, test the viscosity, and discharge the material.

[0092] Comparative Example 5

[0093] (1) Weigh 15 parts of polyether acrylate, 40 parts of polyurethane acrylate and 10 parts of epoxy acrylate respectively, place them in a stirring tank and mix them evenly, add 20 parts of monomer solvent (HEMA) and stir until the oligomer is completely dissolved;

[0094] (2) Weigh 1.5 parts of photoinitiator 784, 0.5 parts of photoinitiator 184, and 2 parts of photoinitiator 819 respectively and place them in a stirring tank, add 5 parts of monomer solvent (HEMA), and stir until the photoinitiators are completely dissolved;

[0095] (3) adding the oligomer dissolved in step (1) to the photoinitiator dissolved in step (2), and stirring at 50° C. for 30 minutes;

[0096] (4) adding 0.5 parts of leveling agent (BYK-UV3510) and 0.5 parts of defoamer (polysiloxane defoamer) to the mixture prepared in step (3), and stirring until completely dissolved;

[0097] (5) After filtering with a sieve, defoam in a vacuum drying oven, test the viscosity, and discharge the material.

[0098] Comparative Example 6

[0099] (1) Weigh 30 parts of polyester acrylate, 10 parts of polyurethane acrylate and 20 parts of epoxy acrylate respectively, place them in a stirring tank and mix them evenly, add 20 parts of monomer solvent (HEMA) and stir until the oligomer is completely dissolved;

[0100] (2) Weigh 1.5 parts of photoinitiator 784, 0.5 parts of photoinitiator 184, and 2 parts of photoinitiator 819 respectively and place them in a stirring tank, add 5 parts of monomer solvent (HEMA), and stir until the photoinitiators are completely dissolved;

[0101] (3) adding the oligomer dissolved in step (1) to the photoinitiator dissolved in step (2), and stirring at 50° C. for 30 minutes;

[0102] (4) adding 0.5 parts of leveling agent (BYK-UV3510) and 0.5 parts of defoamer (polysiloxane defoamer) to the mixture prepared in step (3), and stirring until completely dissolved;

[0103] (5) After filtering with a sieve, defoam in a vacuum drying oven, test the viscosity, and discharge the material.

[0104] Comparative Example 7

[0105] (1) Weigh 15 parts of polyester acrylate, 40 parts of polyurethane acrylate and 10 parts of epoxy acrylate respectively, place them in a stirring tank and mix them evenly, add 20 parts of monomer solvent (HEMA) and stir until the oligomer is completely dissolved;

[0106] (2) Weigh 2 parts of photoinitiator 784, 2 parts of photoinitiator 184, and 1 part of photoinitiator 819 respectively and place them in a stirring tank, add 5 parts of monomer solvent (HEMA), and stir until the photoinitiator is completely dissolved;

[0107] (3) adding the oligomer dissolved in step (1) to the photoinitiator dissolved in step (2), and stirring at 50° C. for 30 minutes;

[0108] (4) adding 0.5 parts of leveling agent (BYK-UV3510) and 0.5 parts of defoamer (polysiloxane defoamer) to the mixture prepared in step (3), and stirring until completely dissolved;

[0109] (5) After filtering with a sieve, defoam in a vacuum drying oven, test the viscosity, and discharge the material.

[0110] Comparative Example 8

[0111] (1) Weigh 15 parts of polyester acrylate, 40 parts of polyurethane acrylate, 10 parts of epoxy acrylate, 1.5 parts of photoinitiator 784, 0.5 parts of photoinitiator 184 and 2 parts of photoinitiator 819 respectively, place them in a stirring tank, add 25 parts of monomer solvent (HEMA), and stir until the photoinitiator and oligomer are completely dissolved;

[0112] (2) adding 0.5 parts of leveling agent (BYK-UV3510) and 0.5 parts of defoamer (polysiloxane defoamer) to the mixture prepared in step (1), and stirring until completely dissolved;

[0113] (3) After filtering with a sieve, defoam in a vacuum drying oven, test the viscosity, and discharge the material.

[0114] Test Example 1

[0115] The nail polish prepared in the above Examples 1 to 6 and Comparative Examples 1 to 6 were brushed on standard nail plates respectively, and placed under LED light to observe their curing conditions; and their viscosity, adhesion and flexibility were tested.

[0116] Viscosity: Tested according to national standard GB / T 265-1988;

[0117] Adhesion: Adhesion is tested according to the national standard GB / T 9286-1998;

[0118] Flexibility: According to the national standard GB / T 1731-1993, the minimum diameter of the shaft corresponding to the paint film not breaking when the paint film is folded in half around the shaft of the shaft rod tester. The smaller the diameter, the greater the bending capacity that the paint film can withstand and the better the flexibility.

[0119] Table 1 Properties of nail polish base materials prepared in various embodiments and comparative examples

[0120]

[0121]

[0122] As shown in Table 1, the nail polish base materials prepared in Examples 1 to 6 of the present invention can be completely cured in only 20 to 40 seconds, while in Comparative Example 2, due to the lack of photoinitiator 819 and the use of only photoinitiator 819 as a photoinitiator in Comparative Example 4, part of the light waves cannot be absorbed, resulting in incomplete curing in 120 seconds; in Comparative Example 7, the dosage of photoinitiator 784 and photoinitiator 184 is relatively high, but the initiation efficiency is low, resulting in incomplete curing in 120 seconds; in Comparative Example 8, due to the direct mixing of multiple substances, the photoinitiator is unevenly distributed, resulting in reduced curing efficiency;

[0123] The flexibility and adhesion of the nail polish base materials prepared in Examples 1 to 6 are relatively strong, while the flexibility and adhesion of the samples prepared in Comparative Examples 1 to 6 are poor;

[0124] The nail polish base materials prepared in Examples 1 to 6 have a viscosity of 4000 to 6000 mPa·s, which is moderate and easy to apply. The nail polish base materials prepared in Comparative Examples 1 to 6 have a viscosity that is too high or too low, which is not easy to apply.

[0125] Although the embodiments of the present invention have been disclosed above, they are not limited to the applications listed in this specification and implementation mode. They can be applied to various fields suitable for the present invention. For those familiar with the art, other modifications can be easily realized. Therefore, without departing from the general concept defined by the claims and equivalent scopes, the present invention is not limited to the specific details listed. The above description is only a preferred embodiment of the present application and an explanation of the technical principles used.

[0126] Those skilled in the art should understand that the scope of the invention involved in this application is not limited to the technical solutions formed by a specific combination of the above-mentioned technical features, but should also cover other technical solutions formed by any combination of the above-mentioned technical features or their equivalent features without departing from the inventive concept.

Claims

1. A visible light-cured nail polish base, characterized in that: The composition comprises the following components by weight: 60-80 parts of oligomer, 3-5 parts of photoinitiator, 15-30 parts of monomer solvent, 0.5-2 parts of leveling agent and 0.5-2 parts of defoaming agent.

2. The visible light-curable nail polish base according to claim 1, characterized in that: The oligomer is composed of polyester acrylate, polyurethane acrylate and epoxy acrylate, and the mass ratio of each component is polyester acrylate: polyurethane acrylate: epoxy acrylate = (5-20): (20-50): (5-10).

3. The visible light-curable nail polish base according to claim 2, characterized in that: The photoinitiators include photoinitiator 784 , photoinitiator 184 and photoinitiator 819 .

4. The visible light-curable nail polish base according to claim 3, characterized in that: The mass ratio of each initiator in the photoinitiator is photoinitiator 784:photoinitiator 184:photoinitiator 819=(0.5-1.5):(0.2-1):(1-3).

5. The visible light-curable nail polish base according to claim 1, characterized in that: The monomer solvent is selected from one or more of hydroxyethyl methacrylate (HEMA), hydroxypropyl methacrylate (HPMA), and butyl acrylate (BA).

6. The visible light-curable nail polish base according to claim 1, characterized in that: The leveling agent is selected from one or more of BYK-UV3510, BYK-341, BYK-344, BYK-345, BYK-346, BYK-347, and BYK-348.

7. The visible light-curable nail polish base according to claim 1, characterized in that: The defoamer is selected from a polysiloxane defoamer and a polyether defoamer.

8. The method for preparing the nail polish base according to any one of claims 1 to 7, characterized in that: The steps include: (1) Weighing a certain amount of polyester acrylate, polyurethane acrylate and epoxy acrylate according to the formula ratio, placing them in a stirring tank and mixing them evenly, adding a portion of the monomer solvent and stirring until the oligomer is completely dissolved; (2) Weigh a certain amount of photoinitiator 784, photoinitiator 184 and photoinitiator 819 according to the formula ratio, place them in a stirring tank, add a portion of the monomer solvent, and stir until the photoinitiator is completely dissolved; (3) adding the oligomer dissolved in step (1) to the photoinitiator dissolved in step (2), and stirring at 50 to 60° C.; (4) adding a leveling agent and a defoaming agent to the mixture prepared in step (3), and stirring until completely dissolved; (5) After filtering with a sieve, defoam in a vacuum drying oven, test the viscosity, and discharge the material.

9. The method for preparing the nail polish base according to claim 8, characterized in that: In step (1), the mass ratio of the monomer solvent used to dissolve the oligomer to the oligomer is (1-2.5):(6-8).

10. The method for preparing the nail polish base according to claim 8, characterized in that: In step (2), the mass ratio of the monomer solvent used to dissolve the photoinitiator to the photoinitiator is 5:(3-5).

Citation Information

Patent Citations

  • Flame retardant ultraviolet-curing decorative adhesive and preparation method thereof

    CN104312454A

  • Fast curing cosmetic compositions for tack free surface photocuring of radically polymerizable resins with uv-led

    CN104519863A

  • Flexible LED nail lacquer gel and preparing method thereof

    CN104921971A

  • Environment-friendly UV nail polish coating composition and preparing method thereof

    CN105030567A

  • High-performance Japanese-style color oil glue and preparation and use methods thereof

    CN110384638A

Cited By

  • Visible light curing-based nail gel base material and preparation method therefor

    WO2026040714A1