Catalyst for preparing 3-cyanopyridine and preparation method thereof
By combining graphene oxide and titanium dioxide composite support with vanadium, molybdenum, antimony and phosphorus-containing compounds, a high-efficiency catalyst was prepared, which solved the problems of low catalyst selectivity and yield in the prior art, and achieved high conversion and high purity 3-cyanopyridine preparation.
Patent Information
- Application Number
- CN202411157611.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, the catalyst for preparing 3-cyanopyridine has low selectivity and low yield, making it difficult to effectively improve the conversion rate of 3-methylpyridine and the purity of 3-cyanopyridine.
A composite support of graphene oxide and titanium dioxide was used to immerse and calcinate with a mixed solution containing vanadium, molybdenum, antimony and phosphorus compounds through hydrothermal reaction to prepare a catalyst with a high active component partition ratio.
The conversion rate of 3-methylpyridine and the selectivity and yield of 3-cyanopyridine were significantly improved, with the conversion rate reaching more than 99%, and the selectivity and yield reaching more than 97.5% and more than 95.4% respectively.
Smart Images

Figure BDA0005006657830000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of organic synthesis catalysts, and in particular to a catalyst for preparing 3-cyanopyridine and a preparation method thereof. Background Art
[0002] 3-Cyanopyridine is an important fine chemical intermediate, widely used in food, medicine and aquaculture. The simplest method for synthesizing 3-cyanopyridine is the 3-methylpyridine gas phase ammoxidation process, which has the advantages of low cost, simple process flow and relatively friendly environment. However, the ammoxidation reaction process is a complicated process. In addition to the main reaction, there are many side reactions, and the difficulty lies in the preparation of the catalyst. The catalyst for the ammoxidation reaction requires not only a high conversion rate, but also a high selectivity.
[0003] CN106111172A discloses a catalyst for catalyzing ammoxidation reaction to prepare 3-cyanopyridine and a preparation method thereof. The catalyst is based on titanium dioxide and vanadium pentoxide. Oxalic acid, tin oxide, cerium oxide, silver oxide, sodium hypophosphite and zinc phosphate are added during the preparation process. After grinding, the catalyst is evenly sprayed on an SMA maleic anhydride catalyst carrier to obtain the catalyst. When catalyzing the ammoxidation reaction, the conversion rate of 3-methylpyridine is up to 96.4%, and the purity of 3-cyanopyridine is up to 96.0%. Therefore, it is of great significance to study a catalyst for preparing 3-cyanopyridine and a preparation method thereof to improve the conversion rate of reaction raw materials and the yield of the product. Summary of the invention
[0004] The object of the present invention is to provide a catalyst for preparing 3-cyanopyridine and a preparation method thereof, so as to solve the problems of low selectivity and low yield in the preparation of 3-cyanopyridine in the prior art.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a catalyst for preparing 3-cyanopyridine, comprising the following steps:
[0007] (1) mixing graphene oxide and a solvent to obtain a graphene oxide dispersion;
[0008] (2) mixing the graphene oxide dispersion and tetrabutyl titanate and performing a hydrothermal reaction to obtain a composite carrier of graphene oxide and titanium dioxide;
[0009] (3) mixing a vanadium-containing compound and water, and then sequentially adding a molybdenum-containing compound, an antimony-containing compound, and a phosphorus-containing compound to obtain a mixed solution;
[0010] (4) After the composite support is formed, it is immersed in the mixed solution, and then dried and calcined in sequence to obtain a catalyst for preparing 3-cyanopyridine.
[0011] Preferably, in step (1), the concentration of graphene oxide in the graphene oxide dispersion is 1 to 5 mg / mL.
[0012] Preferably, in step (2), the volume ratio of the graphene oxide dispersion to tetrabutyl titanate is 1:0.1 to 0.3.
[0013] Preferably, in step (2), the temperature of the hydrothermal reaction is 150-170° C., and the time of the hydrothermal reaction is 1-3 h.
[0014] Preferably, in step (3), the atomic ratio of vanadium in the vanadium-containing compound, molybdenum in the molybdenum-containing compound, antimony in the antimony-containing compound and phosphorus in the phosphorus-containing compound is 1:0.1-0.3:0.05-0.08:0.06-0.012.
[0015] Preferably, in step (3), the mass volume ratio of the vanadium-containing compound to water is 1-3 g: 20-50 mL.
[0016] Preferably, in step (4), the mass volume ratio of the composite carrier to the mixed solution is 15-30 g:50-120 mL.
[0017] Preferably, in the step (4), the impregnation time is 18 to 24 hours; the calcination temperature is 400 to 500° C., and the calcination time is 5 to 8 hours.
[0018] The present invention provides a catalyst for preparing 3-cyanopyridine, which is prepared by the above-mentioned preparation method.
[0019] Beneficial effects of the present invention:
[0020] (1) The catalyst prepared by the composite carrier of graphene oxide and titanium dioxide is used to prepare 3-cyanopyridine, which can not only improve the conversion rate of 3-methylpyridine, but also improve the selectivity and yield of 3-cyanopyridine.
[0021] (2) The present invention can further improve the selectivity and yield of 3-cyanopyridine by controlling the atomic ratio of vanadium, molybdenum, antimony and phosphorus in the active components of the catalyst. DETAILED DESCRIPTION
[0022] The present invention provides a method for preparing a catalyst for preparing 3-cyanopyridine, comprising the following steps:
[0023] (1) mixing graphene oxide and a solvent to obtain a graphene oxide dispersion;
[0024] (2) mixing the graphene oxide dispersion and tetrabutyl titanate and performing a hydrothermal reaction to obtain a composite carrier of graphene oxide and titanium dioxide;
[0025] (3) mixing a vanadium-containing compound and water, and then sequentially adding a molybdenum-containing compound, an antimony-containing compound, and a phosphorus-containing compound to obtain a mixed solution;
[0026] (4) After the composite support is formed, it is immersed in the mixed solution, and then dried and calcined in sequence to obtain a catalyst for preparing 3-cyanopyridine.
[0027] In the present invention, in step (1), the concentration of graphene oxide in the graphene oxide dispersion is 1 to 5 mg / mL, preferably 2 to 4 mg / mL, and more preferably 2 mg / mL.
[0028] In the present invention, the solvent is anhydrous ethanol or ethylene glycol, preferably anhydrous ethanol.
[0029] In the present invention, the graphene oxide and the solvent are preferably mixed and then subjected to ultrasonic treatment, and the ultrasonic treatment time is 30 to 50 minutes, preferably 35 to 45 minutes, and more preferably 40 minutes.
[0030] In the present invention, in step (2), the volume ratio of the graphene oxide dispersion to tetrabutyl titanate is 1:0.1 to 0.3, preferably 1:0.15 to 0.25, and more preferably 1:0.2.
[0031] In the present invention, tetrabutyl titanate is preferably added dropwise to the graphene oxide dispersion, and then ultrasonic treatment is performed after the addition is completed. The ultrasonic treatment time is 30 to 50 minutes, preferably 35 to 45 minutes, and more preferably 40 minutes.
[0032] In the present invention, in step (2), the temperature of the hydrothermal reaction is 150-170°C, preferably 155-165°C, and more preferably 160°C; the time of the hydrothermal reaction is 1-3h, preferably 1.5-2.5h, and more preferably 2h.
[0033] In the present invention, in step (3), the atomic ratio of vanadium in the vanadium-containing compound, molybdenum in the molybdenum-containing compound, antimony in the antimony-containing compound and phosphorus in the phosphorus-containing compound is 1:0.1-0.3:0.05-0.08:0.06-0.012, preferably 1:0.2:0.06-0.07:0.08-0.010, and further preferably 1:0.2:0.06:0.010.
[0034] In the present invention, in step (3), the mass volume ratio of the vanadium-containing compound to water is 1-3 g:20-50 mL, preferably 1.5-2.5 g:30-40 mL, and more preferably 2 g:30 mL.
[0035] In the present invention, in the step (3), the vanadium-containing compound and water are mixed and heated to 70-90° C. for dissolution.
[0036] In the present invention, in the step (4), the composite carrier is formed in a kneader, and the composite carrier is placed in the kneader, and water is added, kneaded, dried, and calcined.
[0037] In the present invention, the specific steps of composite carrier molding are: first, the composite carrier is placed in a kneading machine, and an appropriate amount of water is added for kneading, and the kneading time is 1 to 3 hours, and then the composite carrier is extruded through an extruder, and cut into particles by a cutting machine, and then placed in an oven for drying, and then placed in a muffle furnace for roasting after drying, wherein the roasting temperature is 400 to 600°C, and the roasting time is 1 to 2 hours, to obtain a molded composite carrier with a particle size of 0.3 to 1.0 cm.
[0038] In the present invention, in step (4), the mass volume ratio of the composite carrier to the mixed solution is 15-30 g:50-120 mL, preferably 18-25 g:60-110 mL, and more preferably 20-22 g:80-100 mL.
[0039] In the present invention, in the step (4), the impregnation time is 18 to 24 hours, preferably 19 to 23 hours, and more preferably 20 to 22 hours; the roasting temperature is 400 to 500°C, preferably 420 to 480°C, and more preferably 450°C; the roasting time is 5 to 8 hours, preferably 6 to 7 hours, and more preferably 6 hours.
[0040] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0041] Example 1
[0042] First, 100 mg of graphene oxide was weighed and put into a beaker, and then 100 mL of anhydrous ethanol was added to mix, and after ultrasonic treatment for 30 minutes, a graphene oxide dispersion was obtained, 20 mL of tetrabutyl titanate was added dropwise to the graphene oxide dispersion, and ultrasonic treatment was performed for 40 minutes, and then the dispersion was transferred to a hydrothermal reactor and reacted at a temperature of 160°C for 2 hours. After the reaction was completed, the hydrothermal reaction product was centrifuged, washed, and dried to obtain a composite carrier of graphene oxide and titanium dioxide.
[0043] Add 20 g of ammonium metavanadate to 300 mL of deionized water, heat to 80°C to fully dissolve, then add ammonium molybdate tetrahydrate, and finally add antimony nitrate and potassium dihydrogen phosphate, continue to keep warm and stir until all are dissolved to obtain a mixed solution, ensuring that the atomic ratio of vanadium, molybdenum, antimony and phosphorus in the mixed solution is 1:0.2:0.06:0.010.
[0044] The composite carrier is placed in a kneading machine, and an appropriate amount of water is added for kneading for 2 hours. Then, it is extruded through an extruder, cut into particles with a cutting machine, and then placed in an oven for drying at 100°C. After drying, it is placed in a muffle furnace for calcination, wherein the calcination temperature is 500°C and the calcination time is 2 hours to obtain a formed composite carrier with a particle size range of 0.3 to 1.0 cm.
[0045] 20 g of the formed composite carrier was immersed in 100 mL of the mixed solution at 80°C for 20 h, and then centrifuged. The solid product was dried in a constant temperature drying oven at 80°C for 3 h, and then calcined at 450°C for 6 h to obtain a catalyst for the preparation of 3-cyanopyridine.
[0046] Example 2
[0047] First, 300 mg of graphene oxide was weighed and put into a beaker, and then 100 mL of anhydrous ethanol was added to mix, and after ultrasonic treatment for 40 minutes, a graphene oxide dispersion was obtained, 30 mL of tetrabutyl titanate was added dropwise to the graphene oxide dispersion, and ultrasonic treatment was performed for 50 minutes, and then the dispersion was transferred to a hydrothermal reactor and reacted at a temperature of 150°C for 3 hours. After the reaction, the hydrothermal reaction product was centrifuged, washed, and dried to obtain a composite carrier of graphene oxide and titanium dioxide.
[0048] Add 30 g of ammonium metavanadate to 500 mL of deionized water, heat to 90°C to fully dissolve, then add ammonium molybdate tetrahydrate, and finally add antimony nitrate and potassium dihydrogen phosphate, continue to keep warm and stir until all are dissolved to obtain a mixed solution, ensuring that the atomic ratio of vanadium, molybdenum, antimony and phosphorus in the mixed solution is 1:0.1:0.08:0.006.
[0049] The composite carrier is placed in a kneading machine, and an appropriate amount of water is added for kneading. The kneading time is 3 hours, and then it is extruded through an extruder, cut into particles with a cutting machine, and then placed in an oven for drying at 80°C. After drying, it is placed in a muffle furnace for calcination, wherein the calcination temperature is 400°C and the calcination time is 1 hour to obtain a formed composite carrier with a particle size range of 0.3 to 1.0 cm.
[0050] 30 g of the formed composite carrier was immersed in 120 mL of the mixed solution at 90° C. for 24 h, and then centrifuged. The obtained solid product was dried in a constant temperature drying oven at 80° C. for 3 h, and then calcined at 500° C. for 8 h to obtain a catalyst for the preparation of 3-cyanopyridine.
[0051] Example 3
[0052] First, 500 mg of graphene oxide was weighed and put into a beaker, and then 100 mL of anhydrous ethanol was added to mix, and after ultrasonic treatment for 50 minutes, a graphene oxide dispersion was obtained, 10 mL of tetrabutyl titanate was added dropwise to the graphene oxide dispersion, and ultrasonic treatment was performed for 30 minutes, and then the dispersion was transferred to a hydrothermal reactor and reacted at a temperature of 170°C for 1 hour. After the reaction was completed, the hydrothermal reaction product was centrifuged, washed, and dried to obtain a composite carrier of graphene oxide and titanium dioxide.
[0053] Add 10 g of ammonium metavanadate to 200 mL of deionized water, heat to 70°C to fully dissolve, then add ammonium molybdate tetrahydrate, and finally add antimony nitrate and potassium dihydrogen phosphate, continue to keep warm and stir until all are dissolved to obtain a mixed solution, ensuring that the atomic ratio of vanadium, molybdenum, antimony and phosphorus in the mixed solution is 1:0.3:0.05:0.12.
[0054] The composite carrier is placed in a kneading machine, and an appropriate amount of water is added for kneading. The kneading time is 2 hours, and then it is extruded through an extruder, cut into particles with a cutting machine, and then placed in an oven for drying at a temperature of 110°C. After drying, it is placed in a muffle furnace for calcination, wherein the calcination temperature is 600°C and the calcination time is 2 hours to obtain a formed composite carrier with a particle size range of 0.3 to 1.0 cm.
[0055] 15 g of the formed composite carrier was immersed in 50 mL of the mixed solution at 70°C for 18 h, and then centrifuged. The obtained solid product was dried in a constant temperature drying oven at 80°C for 3 h, and then calcined at 400°C for 5 h to obtain a catalyst for the preparation of 3-cyanopyridine.
[0056] Comparative Example 1
[0057] Add 20 g of ammonium metavanadate to 300 mL of deionized water, heat to 80°C to fully dissolve, then add ammonium molybdate tetrahydrate, and finally add antimony nitrate and potassium dihydrogen phosphate, continue to keep warm and stir until all are dissolved to obtain a mixed solution, ensuring that the atomic ratio of vanadium, molybdenum, antimony and phosphorus in the mixed solution is 1:0.2:0.06:0.010.
[0058] 20 g of the formed titanium dioxide carrier was immersed in 100 mL of the mixed solution at 80°C for 24 hours, and then centrifuged. The solid product was dried in a constant temperature drying oven at 80°C for 3 hours, and then calcined at 450°C for 6 hours to obtain a catalyst for preparing 3-cyanopyridine.
[0059] Comparative Example 2
[0060] The difference from Example 1 is that the amount of graphene oxide used is 80 mg, and other conditions are the same.
[0061] Comparative Example 3
[0062] The difference from Example 1 is that the amount of graphene oxide used is 600 mg, and other conditions are the same.
[0063] Comparative Example 4
[0064] The difference from Example 1 is that antimony nitrate is not added, and other conditions are the same.
[0065] The catalysts prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were used to prepare 3-cyanopyridine. 3-Methylpyridine and water were vaporized at 200° C. in a vaporizer, and then mixed with ammonia and air and introduced into a tubular fixed bed filled with the catalyst at a space velocity of 2500 h -1 , catalyst load is 100 g / (L catalyst h), ammonia is 70 g / h, water is 330 g / h, reaction temperature is 300-320°C, the conversion rate of 3-methylpyridine, selectivity and yield of 3-cyanopyridine are shown in Table 1:
[0066] Table 1 Conversion rate of 3-methylpyridine and selectivity and yield of 3-cyanopyridine
[0067]
[0068]
[0069] As can be seen from Table 1, the present invention adopts a composite carrier of graphene oxide and titanium dioxide, combined with the addition of antimony active ingredients and the control of the ratio of each atom in the active ingredient, which can increase the conversion rate of 3-methylpyridine to more than 99%, the selectivity of the product 3-cyanopyridine can reach more than 97.5%, and the yield of 3-cyanopyridine can reach more than 95.4%.
[0070] As can be seen from the above embodiments, the present invention provides a catalyst for preparing 3-cyanopyridine and a preparation method thereof, firstly mixing graphene oxide and a solvent to obtain a graphene oxide dispersion, then mixing the graphene oxide dispersion and tetrabutyl titanate and performing a hydrothermal reaction to obtain a composite carrier of graphene oxide and titanium dioxide; then mixing a vanadium-containing compound and water, and then sequentially adding a molybdenum-containing compound, an antimony-containing compound, and a phosphorus-containing compound to obtain a mixed solution; finally, the composite carrier is formed and immersed in the mixed solution, and then sequentially dried and calcined to obtain a catalyst for preparing 3-cyanopyridine. The present invention adopts a composite carrier of graphene oxide and titanium dioxide, and by controlling the ratio of each component in the active component, the selectivity and yield of 3-cyanopyridine are improved while ensuring that the conversion rate of 3-methylpyridine is not reduced.
[0071] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a catalyst for preparing 3-cyanopyridine, characterized in that: The steps include: (1) mixing graphene oxide and a solvent to obtain a graphene oxide dispersion; (2) mixing the graphene oxide dispersion and tetrabutyl titanate and performing a hydrothermal reaction to obtain a composite carrier of graphene oxide and titanium dioxide; (3) mixing a vanadium-containing compound and water, and then sequentially adding a molybdenum-containing compound, an antimony-containing compound, and a phosphorus-containing compound to obtain a mixed solution; (4) After the composite support is formed, it is immersed in the mixed solution, and then dried and calcined in sequence to obtain a catalyst for preparing 3-cyanopyridine.
2. The preparation method according to claim 1, characterized in that: In the step (1), the concentration of graphene oxide in the graphene oxide dispersion is 1 to 5 mg / mL.
3. The preparation method according to claim 1 or 2, characterized in that: In the step (2), the volume ratio of the graphene oxide dispersion to tetrabutyl titanate is 1:0.1 to 0.
3.
4. The preparation method according to claim 3, characterized in that: In the step (2), the temperature of the hydrothermal reaction is 150 to 170° C., and the time of the hydrothermal reaction is 1 to 3 hours.
5. The preparation method according to claim 2 or 4, characterized in that: In the step (3), the atomic ratio of vanadium in the vanadium-containing compound, molybdenum in the molybdenum-containing compound, antimony in the antimony-containing compound and phosphorus in the phosphorus-containing compound is 1:0.1-0.3:0.05-0.08:0.06-0.
012.
6. The preparation method according to claim 5, characterized in that: In the step (3), the mass volume ratio of the vanadium-containing compound to water is 1-3 g: 20-50 mL.
7. The preparation method according to claim 2, 4 or 6, characterized in that: In the step (4), the mass volume ratio of the composite carrier to the mixed solution is 15-30 g: 50-120 mL.
8. The preparation method according to claim 7, characterized in that: In the step (4), the impregnation time is 18 to 24 hours; the roasting temperature is 400 to 500° C., and the roasting time is 5 to 8 hours.
9. A catalyst for preparing 3-cyanopyridine obtained by the preparation method according to any one of claims 1 to 8.
Citation Information
Patent Citations
Catalyst for preparing 3-cyanopyridine by catalytic ammoxidation and preparation method thereof
CN106111172A