Wear-resistant material as well as preparation method and application thereof

By mixing molybdenum disulfide lithium-based grease with aluminum powder, magnesium aluminum silicate powder and AlSi12 alloy powder under specific conditions, high temperature and wear-resistant wear materials were prepared, which solved the high temperature environment of TS120A molten iron wheel wear plate The wear problem under the hood has improved the safety and cost-effectiveness of the wear plate.

CN119035537AActive Publication Date: 2024-11-29SGIS SONGSHAN CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411159936.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The existing wear plate materials are severely worn in the high temperature environment of the TS120A molten iron, resulting in high wear rate and driving safety hazards. The existing technology is difficult to fully meet its wear resistance requirements.

Method used

Molybdenum disulfide lithium-based grease is used to mix with aluminum powder, magnesium silicate aluminum powder and AlSi12 alloy powder under specific conditions to prepare high temperature and wear-resistant wear materials. By adjusting the order of raw materials and environmental humidity, we ensure that Optimal wear resistance of materials in high temperature environments.

Benefits of technology

It significantly reduces the wear rate of wear plates, and the wear plate shedding rate is zero, which improves the driving safety of the molten iron truck, reduces the cost of purchasing wear plates, and is suitable for large-scale promotion and application.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

According to the wear-resistant material and the preparation method and application thereof, the molybdenum disulfide lithium-based lubricating grease is sequentially mixed with the aluminum powder, the magnesium aluminum silicate powder and the AlSi12 alloy powder under the specific condition, the wear-resistant material for the TS120A hot metal car wearing plate is prepared, the cost for purchasing and processing the wearing plate is greatly reduced, driving safety of a hot metal car is achieved, and the wear-resistant material is suitable for large-scale popularization and application. The method is suitable for large-scale popularization and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of materials, and in particular to a wear-resistant material and a preparation method and application thereof. Background Art

[0002] TS120A hot metal car is an important hot metal transportation equipment for local steel enterprises. The hot metal car is mainly composed of a frame, a wheel set, an axle box spring device and a basic automatic device. The car adopts an inclined wedge vibration reduction device, which can reduce and avoid the axle box spring, upper center plate and other parts from being subjected to strong impact during operation, and is an important component to maintain the smooth operation of the vehicle. The wear plate on the inclined wedge of the car is installed on the inclined wedge through a positioning boss and a cotter pin. The vibration generated during the operation of the vehicle causes the axle box and the wear plate on the inner guide frame to move relative to the wear plate on the inclined wedge and do work, converting the vibration into heat energy. Long-term operation will cause the wear plate on the axle box, inner guide frame and inclined wedge to wear and produce grooves, and even cause the wear plate to fall off, posing a great hidden danger to driving safety.

[0003] In order to reduce the loss of the wear plate, manufacturers generally replace the wear plate and apply lubricating grease to reduce the friction coefficient between the wear plate on the inner guide frame and the wear plate on the wedge, thereby reducing the loss of the wear plate.

[0004] When the TS120A molten iron car works in a high temperature (60-70°C) environment, ordinary lubricating grease will gradually liquefy and peel off from the wear plate for more than 30 minutes. The wear limit rate of the wear plate of the TS120A molten iron car during one maintenance period is greater than 96%.

[0005] CN102050128A discloses a polymer composite side bearing wear plate, the main body of which is a double-layer structure, the upper layer is a wear-resistant layer made of wear-resistant material, and the lower layer is a reinforcing layer made of glass fiber reinforced plastic material; the wear-resistant material is made of the following raw materials in parts by weight: 12-22 parts of sepiolite fiber, 4-6 parts of glass fiber, 6-10 parts of kaolin, 1.5-2.5 parts of aramid fiber, 5-9 parts of graphite particles, 1.5-2.5 parts of copper fiber, 0.5-1.5 parts of titanium stone powder, 3-5 parts of flake graphite, 4-8 parts of bauxite and 0.5-1.5 parts of inorganic composite fiber. The friction coefficient of the polymer composite side bearing wear plate changes little under the influence of temperature and humidity, and the friction coefficient is stable, which is conducive to improving the stability of the elastic side bearing rotation resistance torque, and further improving the stability and reliability of the running performance of heavy-loaded and speed-up trucks.

[0006] CN101293997A discloses a railway freight car slideway wear plate material, which is composed of a blend of multiple nylon materials, and the weight ratio of each component is: nylon 6: 20-25 parts; nylon 66: 70-80 parts; nylon 12: 15-20 parts; nylon 1010: 30-40 parts. The slideway wear plate made of this material has strength, rigidity and friction performance that can fully meet the use requirements of freight cars.

[0007] CN110305478A discloses a wear-resistant material and a preparation method thereof and a wear-resistant part. The wear-resistant material comprises the following raw materials in parts by weight: 70 to 90 parts of polyamide, 10 to 30 parts of polyether polyurethane, 20 to 30 parts of toughening agent, 5 to 15 parts of plant fiber, 1 to 3 parts of wear-resistant agent, 0.2 to 0.8 parts of cross-linking agent and 0.1 to 0.3 parts of antioxidant.

[0008] However, the above-mentioned wear plate materials are not fully applicable to the TS120A molten iron car, and their wear resistance needs to be further improved. Summary of the invention

[0009] In order to solve the above technical problems, the present invention provides a wear-resistant material and a preparation method and use thereof. By mixing molybdenum disulfide lithium-based grease with aluminum powder, magnesium aluminum silicate powder and AlSi12 alloy powder in sequence under specific conditions, a wear-resistant material for TS120A molten iron car wear plate is prepared; the wear-resistant material is resistant to high temperature and wear, and has a prospect of large-scale promotion and application.

[0010] To achieve this object, the present invention adopts the following technical solutions:

[0011] In a first aspect, the present invention provides a method for preparing a wear-resistant material, the preparation method comprising the following steps:

[0012] (1) molybdenum disulfide lithium-based grease and aluminum powder are first mixed to obtain a first mixed grease;

[0013] (2) The first mixed grease and the magnesium aluminum silicate powder in step (1) are mixed for a second time to obtain a second mixed grease;

[0014] (3) in step (2), the second mixed grease and the AlSi12 alloy powder are mixed for the third time and then cooled to obtain the wear-resistant material;

[0015] The ambient humidity during the mixing process of steps (1) to (3) is 10% RH to 20% RH.

[0016] The preparation method of the wear-resistant material of the present invention is simple to operate, and adopts high temperature resistant molybdenum disulfide lithium-based grease as a base, and sequentially mixes with aluminum powder, magnesium aluminum silicate powder and AlSi12 alloy powder under an ambient humidity of 10% RH to 20% RH to obtain a high temperature resistant and wear resistant wear-resistant material. When the ambient humidity is low during the mixing process, powder agglomeration will occur; when the ambient humidity is high during the mixing process, additional dehumidification equipment needs to be installed to make the ambient humidity meet the requirements, which will increase the preparation cost of the wear-resistant material.

[0017] The role of the raw aluminum powder of the present invention is to increase the friction coefficient without wearing the wear plate by utilizing the lower hardness of aluminum powder than the wear plate. The role of magnesium silicate aluminum powder is to utilize its excellent adsorption performance and protective colloid activity to reduce the tendency of the emulsion to become thin or destroyed when the temperature rises, and can stabilize grease and emulsions containing anionic or non-ionic surfactants. It can also provide spreadability, increase viscosity and film-forming properties. AlSi12 alloy powder is selected instead of other types of alloy powder because AlSi12 alloy powder has the advantages of high wear resistance and small thermal expansion coefficient. When any one of the powders is missing, the wear resistance of the prepared wear-resistant material will decrease. The purpose of adding the aluminum powder, magnesium aluminum silicate powder and AlSi12 alloy powder in sequence for mixing in the present invention is that the wear-resistant material has the best anti-wear performance under a high temperature environment (60-70°C). When the order of adding the raw materials is adjusted, that is, molybdenum disulfide lithium-based grease and magnesium aluminum silicate powder are mixed first, then aluminum powder is added for mixing, and finally AlSi12 alloy powder is added for mixing, the ductility of the wear-resistant material will be reduced.

[0018] The ambient humidity during the mixing process of steps (1) to (3) of the present invention is 10% RH to 20% RH, for example, it can be 10% RH, 12% RH, 14% RH, 15% RH, 18% RH or 20% RH, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0019] Preferably, the mass ratio of the molybdenum disulfide lithium-based grease, aluminum powder, magnesium aluminum silicate powder and AlSi12 alloy powder is (55-65):(15-25):(13-23):(1-7), for example, it can be 55:15:13:1, 58:17:14:2, 60:20:18:2, 62:21:20:5, 64:23:21:6 or 65:25:23:7, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable; preferably it is 60:20:18:2.

[0020] The present invention preferably has a mass ratio of molybdenum disulfide lithium-based grease, aluminum powder, magnesium aluminum silicate powder and AlSi12 alloy powder of (55-65): (15-25): (13-23): (1-7), which has the advantage of excellent anti-wear performance under high temperature environment. When the content of molybdenum disulfide lithium-based grease is low, the adsorption energy absorption will decrease and it will fall off the wear plate; when the content of molybdenum disulfide lithium-based grease is high, the film-forming performance will decrease.

[0021] Preferably, the particle size of the aluminum powder in step (1) is 30 μm to 50 μm, for example, 30 μm, 32 μm, 35 μm, 40 μm, 45 μm or 50 μm, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0022] Preferably, the temperature of the first mixing in step (1) is 90°C to 95°C, for example, it can be 90°C, 90.5°C, 91°C, 92°C, 93°C, 94°C or 95°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0023] The present invention preferably has a temperature of 90°C to 95°C for improving ductility. When the temperature of the first mixing is high, the film forming performance will decrease; when the temperature of the first mixing is low, the ductility will decrease. The temperature of the first mixing of 90°C to 95°C is higher than the temperature of the second mixing of 70°C to 75°C because the aluminum powder and the aluminum magnesium silicate powder have different optimal ductility temperatures when mixed.

[0024] Preferably, the first mixing is followed by stirring for 30 to 60 seconds, for example, 30 seconds, 35 seconds, 40 seconds, 45 seconds, 50 seconds, 55 seconds or 60 seconds, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0025] Preferably, the particle size of the magnesium aluminum silicate powder in step (2) is 500-600 mesh, for example, 500 mesh, 510 mesh, 530 mesh, 550 mesh, 580 mesh or 600 mesh, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] Preferably, the temperature of the second mixing in step (2) is 70°C to 75°C, for example, 70°C, 72°C, 73°C, 74°C or 75°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0027] Preferably, the second mixing is stirred for 90 to 120 seconds, for example, 90 seconds, 95 seconds, 100 seconds, 105 seconds, 110 seconds or 120 seconds, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0028] Preferably, the particle size of the AlSi12 alloy powder in step (3) is 400-500 mesh, for example, it can be 400 mesh, 420 mesh, 450 mesh, 470 mesh, 480 mesh or 500 mesh, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0029] Preferably, the temperature of the third mixing is 110°C to 120°C, for example, 110°C, 112°C, 115°C, 118°C or 120°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0030] The preferred temperature of the third mixing of the present invention is 110°C to 120°C, which has the effect of increasing the fluidity of the anti-wear material. When the temperature of the third mixing is high, the air tightness is too low and the fluidity is too high; when the temperature of the third mixing is low, the air tightness of the anti-wear material is too high and the fluidity is reduced.

[0031] Preferably, the third mixing is followed by stirring for 10 to 30 seconds, for example, 10 seconds, 15 seconds, 20 seconds, 25 seconds, 28 seconds or 30 seconds, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0032] Preferably, the cooling temperature is 26-45°C, for example, 26°C, 28°C, 30°C, 35°C, 40°C or 45°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] As a preferred technical solution of the present invention, the preparation method comprises the following steps:

[0034] (1) Molybdenum disulfide lithium-based grease and aluminum powder with a particle size of 30 μm to 50 μm are first mixed at a temperature of 90° C. to 95° C. and then stirred for 30 to 60 seconds to obtain a first mixed grease;

[0035] (2) in step (1), the first mixed grease and the magnesium aluminum silicate powder with a particle size of 500 to 600 mesh are mixed at a temperature of 70° C. to 75° C. and stirred for 90 to 120 seconds to obtain a second mixed grease;

[0036] (3) Step (2) The second mixed grease and the AlSi12 alloy powder with a particle size of 400-500 mesh are mixed at a temperature of 110° C. to 120° C., stirred for 10-30 seconds, and cooled at a temperature of 26-45° C. to obtain the wear-resistant material;

[0037] The ambient humidity during the mixing process of steps (1) to (3) is 10% RH to 20% RH;

[0038] The mass ratio of the molybdenum disulfide lithium-based grease, aluminum powder, magnesium aluminum silicate powder and AlSi12 alloy powder is (55-65):(15-25):(13-23):(1-7).

[0039] In a second aspect, the present invention further provides a wear-resistant material prepared by the method for preparing the wear-resistant material as described in the first aspect.

[0040] The wear-resistant material of the present invention can be used in a high temperature environment of 60 to 70° C. and has a good wear resistance effect.

[0041] In a third aspect, the present invention further provides a use of the wear-resistant material as described in the second aspect, wherein the wear-resistant material is used for a wear plate of a TS120A molten iron car.

[0042] The wear-resistant material of the present invention is used for the wear plate of TS120A hot metal car. During one repair period, the wear limit rate is less than 2%, and the wear plate shedding rate is zero. This not only greatly reduces the cost of purchasing and processing the wear plate, but also solves the driving hidden dangers of TS120A hot metal car caused by the wear plate over-limit wear, and realizes the essentialization of equipment safety.

[0043] Compared with the prior art, the present invention has at least the following beneficial effects:

[0044] The preparation method of the wear-resistant material provided by the invention is simple to operate, and the prepared wear-resistant material has a good effect of being used for the wear plate of TS120A molten iron car, reduces the cost of purchasing the wear plate, ensures the driving safety of the molten iron car, and is suitable for large-scale promotion and application. DETAILED DESCRIPTION

[0045] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0046] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0047] The following are typical but non-limiting embodiments of the present invention:

[0048] Example 1

[0049] This embodiment provides a method for preparing a wear-resistant material, the preparation method comprising the following steps:

[0050] (1) molybdenum disulfide lithium-based grease and aluminum powder with a particle size of 50 μm are first mixed at a temperature of 95° C. and then stirred for 60 seconds to obtain a first mixed grease;

[0051] (2) in step (1), the first mixed grease and the magnesium aluminum silicate powder with a particle size of 500 mesh are mixed at a temperature of 70° C. and stirred for 120 seconds to obtain a second mixed grease;

[0052] (3) Step (2) The second mixed grease and the AlSi12 alloy powder with a particle size of 500 mesh are mixed at a temperature of 110° C., stirred for 30 seconds, and cooled to a temperature of 45° C. to obtain the wear-resistant material;

[0053] The ambient humidity during the mixing process of steps (1) to (3) is 20% RH;

[0054] The mass ratio of the molybdenum disulfide lithium-based grease, aluminum powder, magnesium aluminum silicate powder and AlSi12 alloy powder is 60:20:18:2.

[0055] Example 2

[0056] This embodiment provides a method for preparing a wear-resistant material, the preparation method comprising the following steps:

[0057] (1) molybdenum disulfide lithium-based grease and aluminum powder with a particle size of 40 μm are first mixed at a temperature of 90° C. and then stirred for 50 seconds to obtain a first mixed grease;

[0058] (2) in step (1), the first mixed grease and the magnesium aluminum silicate powder with a particle size of 600 mesh are mixed at a temperature of 75° C. and stirred for 90 seconds to obtain a second mixed grease;

[0059] (3) Step (2) The second mixed grease and the AlSi12 alloy powder with a particle size of 400 mesh are mixed at a temperature of 120° C., stirred for 10 seconds, and cooled to a temperature of 26° C. to obtain the wear-resistant material;

[0060] The ambient humidity during the mixing process of steps (1) to (3) is 10% RH;

[0061] The mass ratio of the molybdenum disulfide lithium-based grease, aluminum powder, magnesium aluminum silicate powder and AlSi12 alloy powder is 55:25:13:7.

[0062] Example 3

[0063] This embodiment provides a method for preparing a wear-resistant material, the preparation method comprising the following steps:

[0064] (1) molybdenum disulfide lithium-based grease and aluminum powder with a particle size of 30 μm are first mixed at a temperature of 92° C. and then stirred for 30 seconds to obtain a first mixed grease;

[0065] (2) The first mixed grease and the magnesium aluminum silicate powder with a particle size of 550 mesh in step (1) are mixed at a temperature of 72° C. and stirred for 100 seconds to obtain a second mixed grease;

[0066] (3) In step (2), the second mixed grease and the AlSi12 alloy powder with a particle size of 460 mesh are mixed at a temperature of 113° C., stirred for 20 seconds, and cooled at a temperature of 30° C. to obtain the wear-resistant material;

[0067] The ambient humidity during the mixing process of steps (1) to (3) is 12% RH;

[0068] The mass ratio of the molybdenum disulfide lithium-based grease, aluminum powder, magnesium aluminum silicate powder and AlSi12 alloy powder is 65:15:19:1.

[0069] Example 4

[0070] The present embodiment provides a method for preparing a wear-resistant material. The preparation method is the same as that of Example 1, except that the mass ratio of the molybdenum disulfide lithium-based grease, aluminum powder, magnesium aluminum silicate powder and AlSi12 alloy powder is 50:30:18:2.

[0071] Example 5

[0072] The present embodiment provides a method for preparing a wear-resistant material. The preparation method is the same as that of Example 1, except that the mass ratio of molybdenum disulfide lithium-based grease, aluminum powder, magnesium aluminum silicate powder and AlSi12 alloy powder is 70:10:18:2.

[0073] Example 6

[0074] This embodiment provides a method for preparing a wear-resistant material. The preparation method is the same as that of Embodiment 1 except that the temperature of the first mixing is 80°C.

[0075] Example 7

[0076] This embodiment provides a method for preparing a wear-resistant material. The preparation method is the same as that of Embodiment 1 except that the temperature of the first mixing is 100°C.

[0077] Comparative Example 1

[0078] This comparative example provides a method for preparing a wear-resistant material. The preparation method is the same as Example 1 except that the order of step (1) and step (2) is changed, that is, molybdenum disulfide lithium-based grease and magnesium silicate aluminum powder with a particle size of 500 mesh are mixed at a temperature of 70°C and then stirred for 120s, and then mixed with aluminum powder with a particle size of 50 μm at a temperature of 95°C.

[0079] The wear-resistant material prepared in the above embodiments and comparative examples was applied to the wear plate of the TS120A molten iron car with a thickness of 2 mm, and a wear resistance test was carried out in an environment of 60-70°C. The results of the wear plate over-limit rate and the wear plate shedding rate within one repair period are shown in Table 1.

[0080] Table 1

[0081] Wear plate wear excess rate (%) Wear plate shedding rate (%) Example 1 0.08% 0 Example 2 0.05% 0 Example 3 0.01% 0 Example 4 6% 9% Example 5 0.75% 11% Example 6 0.9% 11% Example 7 1% 12%

[0082] From Table 1 we can see that:

[0083] (1) It can be seen from Examples 1 to 3 that the preparation method of the wear-resistant material provided by the present invention is simple to operate. When the prepared wear-resistant material is applied to the wear plate of a TS120A molten iron car, the wear limit rate of the wear plate is less than 2%, and the wear plate shedding rate is zero;

[0084] (2) It can be seen from the combination of Example 1 and Examples 4 to 5 that the content of molybdenum disulfide lithium-based grease in Example 4 is relatively low, resulting in an increase in the wear plate wear limit rate of 6% and an increase in the wear plate shedding rate of 9%; the content of molybdenum disulfide lithium-based grease in Example 5 is relatively high, resulting in an increase in the wear plate wear limit rate of 0.75% and an increase in the wear plate shedding rate of 11%.

[0085] (3) Combining Example 1 with Examples 6 and 7, it can be seen that the temperature of the first mixing in Example 6 is relatively low, resulting in an increase in the wear plate over-limit rate to 0.9% and an increase in the wear plate shedding rate to 11%. The temperature of the first mixing in Example 7 is relatively high, resulting in an increase in the wear plate over-limit rate to 1% and an increase in the wear plate shedding rate to 12%.

[0086] (4) It can be seen from Example 1 and Comparative Example 1 that in Comparative Example 1, the molybdenum disulfide lithium-based grease and magnesium aluminum silicate powder are mixed, and then aluminum powder is added for mixing, and finally AlSi12 alloy powder is added for mixing, which will lead to a decrease in the ductility of the wear-resistant material.

[0087] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a wear-resistant material, characterized in that: The preparation method comprises the following steps: (1) molybdenum disulfide lithium-based grease and aluminum powder are first mixed to obtain a first mixed grease; (2) The first mixed grease and the magnesium aluminum silicate powder in step (1) are mixed for a second time to obtain a second mixed grease; (3) Step (2) The second mixed grease and AlSi12 alloy powder are mixed for the third time and then cooled to obtain the wear-resistant material; The ambient humidity during the mixing process of steps (1) to (3) is 10% RH to 20% RH.

2. The preparation method according to claim 1, characterized in that: The mass ratio of the molybdenum disulfide lithium-based grease, aluminum powder, magnesium aluminum silicate powder and AlSi12 alloy powder is (55-65):(15-25):(13-23):(1-7), preferably 60:20:18:

2.

3. The preparation method according to claim 1 or 2, characterized in that: The particle size of the aluminum powder in step (1) is 30 μm to 50 μm.

4. The preparation method according to any one of claims 1 to 3, characterized in that: Step (1) The temperature of the first mixing is 90° C. to 95° C.; Preferably, the first mixing is followed by stirring for 30 to 60 seconds.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The particle size of the magnesium aluminum silicate powder in step (2) is 500-600 mesh.

6. The preparation method according to any one of claims 1 to 5, characterized in that: Step (2) the temperature of the second mixing is 70°C to 75°C; Preferably, the second mixing is followed by stirring for 90 to 120 seconds.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The particle size of the AlSi12 alloy powder in step (3) is 400-500 mesh; Preferably, the temperature of the third mixing is 110°C to 120°C; Preferably, the third mixing is followed by stirring for 10 to 30 seconds; Preferably, the cooling temperature is 26-45°C.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: (1) Molybdenum disulfide lithium-based grease and aluminum powder with a particle size of 30 μm to 50 μm are first mixed at a temperature of 90° C. to 95° C. and then stirred for 30 to 60 seconds to obtain a first mixed grease; (2) in step (1), the first mixed grease and the magnesium aluminum silicate powder with a particle size of 500 to 600 mesh are mixed at a temperature of 70° C. to 75° C. and stirred for 90 to 120 seconds to obtain a second mixed grease; (3) Step (2) The second mixed grease and the AlSi12 alloy powder with a particle size of 400-500 mesh are mixed at a temperature of 110° C. to 120° C., stirred for 10-30 seconds, and cooled at a temperature of 26-45° C. to obtain the wear-resistant material; The ambient humidity during the mixing process of steps (1) to (3) is 10% RH to 20% RH; The mass ratio of the molybdenum disulfide lithium-based grease, aluminum powder, magnesium aluminum silicate powder and AlSi12 alloy powder is (55-65):(15-25):(13-23):(1-7).

9. A wear-resistant material prepared by the method for preparing a wear-resistant material according to any one of claims 1 to 8.

10. Use of the wear-resistant material according to claim 9, characterized in that: The wear-resistant material is used for the wear plate of TS120A hot metal car.

Citation Information

Patent Citations

  • Goods train sliding chute wear plate material

    CN101293997A

  • Polymer composite side bearing wear plate

    CN102050128A

  • Abrasion-resistant material, preparation method of abrasion-resistant material and abrasion-resistant part

    CN110305478A

  • Plastic sliding bearing wear-resistant material and preparation method thereof

    CN106633851A

  • Preparation method of quaternary ammonium salt modified organic magnesium aluminosilicate for thickening oily system

    CN108706605A