Fireproof and wear-resistant thermal insulation composite board and preparation method thereof
By introducing dynamic thiocarbamate and modified inorganic fillers into polyurethane adhesives, and utilizing the reaction between polyimide and aluminum dihydrogen phosphate in flame-retardant insulation materials to form an inorganic protective layer, the problems of flammability, poor fire resistance, and poor wear resistance of polyurethane composite boards are solved, thereby improving fire resistance and wear resistance.
Patent Information
- Application Number
- CN202411527808.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-10-30
AI Technical Summary
In existing technologies, when polyurethane and other polymer materials are combined with metal plates, the resulting metal composite plates suffer from problems such as flammability, poor fire resistance, and poor wear resistance.
The composite structure consists of a flame-retardant insulation layer, a first wear-resistant layer, and a second wear-resistant layer. By introducing dynamic thiocarbamate and modified inorganic fillers into the polyurethane adhesive, and reacting with the polyimide and aluminum dihydrogen phosphate of the flame-retardant insulation material, an inorganic protective layer is formed, which improves the fire resistance and wear resistance.
It significantly improves the fire resistance and wear resistance of polyurethane composite panels, possesses good self-healing properties and flame retardant effect, and reduces heat release and thermal conductivity during combustion.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite board materials, and in particular to a fireproof and wear-resistant thermal insulation composite board and a preparation method thereof. Background Art
[0002] One of the main problems facing mankind today is the energy problem. Building energy consumption accounts for a large proportion of the total social energy consumption. Most buildings in my country have extremely low energy utilization rates and are high-energy-consuming buildings. Therefore, building energy conservation is one of the most effective ways to save energy, which is conducive to alleviating the current situation of insufficient energy supply and improving the environment to achieve sustainable development. Polyurethane has excellent mechanical strength, waterproof properties and low thermal conductivity, and is an excellent thermal insulation material. The metal composite panel obtained by compounding metal plates and polyurethane materials is an ideal ultra-low energy consumption building material. However, as an organic polymer material, polyurethane has technical problems such as flammability and poor wear resistance.
[0003] Patent application CN113292924A discloses a method for preparing a heat-insulating and wear-resistant composite plate, wherein the heat-resistant and wear-resistant composite plate includes a substrate, a wear-resistant alloy plate, a heat-resistant adhesive layer and a wear-resistant coating; wherein the heat-resistant adhesive layer is composed of silicon boron rubber, epoxy resin, modified nano antimony tin oxide, modified nano boron nitride, etc., and the wear-resistant coating is composed of modified silicon carbide whiskers, modified nano titanium diboride, epoxy resin, etc., and the above-mentioned prior art utilizes various inorganic materials to improve the heat resistance and wear resistance of the composite plate, but epoxy resin, as an organic polymer material, has poor wear resistance itself and fails to significantly improve the fire resistance and wear resistance of the base resin material itself.
[0004] Patent application CN112695179A discloses a method for preparing a graphene metal composite plate, which comprises evenly applying melted graphene on the outer surface of a metal plate, and then laminating the two sides of the metal plates coated with graphene to each other, thereby preparing a graphene metal composite plate; however, the connection process of the above-mentioned graphene metal composite plate consumes too much energy, and the above-mentioned composite metal plate only improves its own fire resistance and wear resistance by graphene, resulting in poor fire resistance, heat preservation and wear resistance of the prepared metal composite plate.
[0005] In view of the technical defects in this aspect, a solution is now proposed. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing a fireproof and wear-resistant thermal insulation composite board, which is used to solve the technical problem in the prior art that after a polymer material such as polyurethane is composited with a metal plate, the organic layer of the metal composite board is flammable, has poor fire resistance and poor wear resistance.
[0007] The purpose of the present invention can be achieved through the following technical solutions: A fireproof and wear-resistant thermal insulation composite panel, comprising a pretreated metal substrate A, a first wear-resistant layer, a flame-retardant thermal insulation layer, a second wear-resistant layer and a pretreated metal substrate B arranged in sequence from bottom to top; The flame retardant thermal insulation layer is prepared from a flame retardant thermal insulation material; The first wear-resistant layer and the second wear-resistant layer are both prepared from a wear-resistant adhesive; The preparation method of the wear-resistant adhesive is as follows: isophorone diisocyanate, 2-mercaptopropionic acid, diol and modified inorganic filler are mixed, mixed and reacted at 70-80° C. for 30 minutes under a nitrogen atmosphere, and then a catalyst is added, and the reaction is continued at 70-80° C. for 4-5 hours to obtain a reaction product; the reaction product is cooled to room temperature, and then a neutralizer is added, and continuous stirring is performed, and deionized water is added dropwise for emulsification to obtain a wear-resistant adhesive layer.
[0008] The wear-resistant adhesive prepared by the present invention is a polyurethane resin; specifically, isophorone diisocyanate provides -NCO, and under the action of a catalyst dibutyltin dilaurate, an isocyanate group and a hydroxyl group of a diol react to generate carbamate, thereby obtaining a wear-resistant adhesive; and when synthesizing a polyurethane prepolymer, 2-mercaptopropionic acid is added, and the isocyanate group reacts with the mercapto group in the 2-mercaptopropionic acid, and dynamic thiocarbamate is introduced into the main chain of the polyurethane, thereby adding self-repairing properties to the wear-resistant adhesive layer.
[0009] Furthermore, the modified inorganic filler is prepared by the following steps: The tris(hydroxymethyl)aminomethane) powder and deionized water are mixed evenly to obtain a tris(hydroxymethyl)aminomethane buffer solution; the spherical alumina is passed through a 100-mesh sieve to obtain a spherical alumina powder; the tris(hydroxymethyl)aminomethane buffer solution, the spherical alumina powder and dopamine hydrochloride are mixed and stirred at 100 r / min for 24 hours, and then filtered to obtain a solid material; the solid material is washed with deionized water, and then dried at 60-70° C. for 24 hours to obtain a modified inorganic filler.
[0010] The aqueous solution of tris(hydroxymethylaminomethane) is used as a buffer solution, and the aluminum oxide is organically modified by dopamine hydrochloride to obtain the aluminum oxide coated with dopamine hydrochloride, thereby realizing the organic modification of the aluminum oxide.
[0011] Furthermore, the usage ratio of tris(hydroxymethyl)aminomethane powder and deionized water is 10-15 g:100 mL; the usage ratio of tris(hydroxymethyl)aminomethane buffer solution, spherical alumina powder and dopamine hydrochloride is 5-10 g:0.5 g:100 mL.
[0012] Furthermore, the diol is any one of ethylene glycol, 1,4-butanediol, 1,2-propylene glycol, methylpropylene glycol and a combination thereof, the catalyst is dibutyltin dilaurate, and the neutralizer is ethylenediamine; the dosage ratio of isophorone diisocyanate, 2-mercaptopropionic acid, diol, modified inorganic filler, catalyst and neutralizer is 20-30g:5-10g:60g:5-10g:0.01g:2-5g; the rotation speed of the mixing reaction is 100-120r / min, and the rotation speed of continuous stirring is 1000r / min.
[0013] Furthermore, the flame retardant heat-insulating material is prepared by the following steps: S1. Mix dimethyldichlorosilane, ethylenediamine and dioxane, stir at 60-70°C for 2h, then heat to 90°C, mix and react for 2h to obtain intermediate product A; add cyanuric chloride to intermediate product A, react at 0°C for 2-3h, then heat to 50°C, mix and react for 2-3h; then heat to 100°C, continue to react for 2-3h to obtain a product; add the product to deionized water, filter and obtain a product; grind and crush the product, pass through a 100-mesh sieve to obtain a flame retardant material; S2. Mix phosphoric acid and aluminum hydroxide to obtain aluminum dihydrogen phosphate solution; mix the flame retardant material and the aluminum dihydrogen phosphate solution to react, and then filter to obtain a solid; vacuum dry the solid at 60-70° C. for 30 minutes to obtain a flame retardant thermal insulation material.
[0014] The synthesis principle of intermediate product A is as follows:
[0015] The synthesis principle of flame retardant materials is as follows:
[0016] Using dioxane as an organic solvent, dimethyldichlorosilane and ethylenediamine undergo a substitution reaction, and then react with cyanuric chloride to obtain a flame retardant material rich in flame retardant elements silicon and nitrogen.
[0017] Aluminum hydroxide reacts with phosphoric acid to generate aluminum dihydrogen phosphate, and the flame retardant thermal insulation material is obtained by utilizing the adsorption reaction between the polyimide group of the flame retardant material and the phosphate radical of the aluminum dihydrogen phosphate.
[0018] Furthermore, in step S1, the dosage ratio of dimethyldichlorosilane, ethylenediamine, dioxane, cyanuric chloride and deionized water is 12-15mL:5-10g:250mL:15-20g:100mL; the rotation speed of the mixed reaction is 100-200r / min, and the rotation speed of the continuous reaction is 100-200r / min.
[0019] Furthermore, in step S2, the dosage ratio of phosphoric acid and aluminum hydroxide is 30mL:10-15g; the rotation speed of the mixing reaction is 100r / min, and the duration of the mixing reaction is 30min; the dosage ratio of the flame retardant material and the dialuminum dihydrogen phosphate solution is 10-20g:10mL.
[0020] The present invention also provides a method for preparing a fireproof and wear-resistant thermal insulation composite board, comprising the following steps: A1. Grinding the surface of the metal substrate with a grinding wheel at a speed of 10 m / s for 5-10 min to obtain a polished metal substrate; ultrasonically cleaning the polished metal substrate with a degreasing agent as a cleaning liquid, the frequency of ultrasonic cleaning is 16-20 kHz, and the duration of ultrasonic cleaning is 10-20 min to obtain a pretreated metal composite plate; The present invention selects an aluminum-zinc-plated substrate as a metal substrate, uses a polishing tool to level the surface of the metal substrate, and then uses a degreasing agent to degrease the surface of the metal substrate; under the action of ultrasonic waves, ultrasonic cleaning uses longitudinal waves to drive the cleaning liquid, so that the liquid produces countless tiny vacuum bubbles. When the bubbles are compressed and exploded, powerful shock waves are generated to flush the oil stains, thereby obtaining a metal substrate that has been pre-treated with a deoiled and degreased surface.
[0021] A2. Coat one side of the pretreated metal substrate A with a wear-resistant adhesive to obtain a first wear-resistant layer; spread a flame-retardant thermal insulation material on the surface of the first wear-resistant layer to obtain a flame-retardant thermal insulation layer; coat the surface of the flame-retardant thermal insulation layer with a wear-resistant adhesive layer to obtain a second wear-resistant layer; then place the pretreated metal substrate B to obtain a metal composite plate; dry the metal composite plate at room temperature for 24 hours, then dry it in a vacuum environment of 70-80°C for 24 hours, and then braze the pretreated metal substrate A and the pretreated metal substrate B to obtain a fire-resistant and wear-resistant thermal insulation composite plate.
[0022] Furthermore, the pretreated metal substrate is an aluminum-zinc-plated substrate; the thickness of the first wear-resistant adhesive layer and the second wear-resistant adhesive layer are both 10-20 μm, and the thickness of the flame-retardant thermal insulation layer is 10-20 μm.
[0023] The present invention has the following beneficial effects: 1. The wear-resistant adhesive layer of the composite plate prepared by the present invention is actually a polyurethane adhesive. When synthesizing the polyurethane adhesive, 2-mercaptopropionic acid is added to introduce dynamic thiocarbamate on the main chain of the polyurethane, which gives the wear-resistant adhesive layer good self-repairing properties without affecting the original network structure of the polyurethane, thereby improving the wear resistance of the wear-resistant adhesive. However, as an organic substance, polyurethane is flammable. In addition, the mechanical properties of polyurethane adhesives are weak; when preparing the wear-resistant adhesive layer, the present invention adds a modified inorganic filler as a reinforcing material for the polyurethane adhesive; the inorganic material alumina is selected to be spherical, the surface area of spherical alumina is the smallest, the isotropy is good, and it is uniformly stirred with polyurethane to form a film, and it will have excellent fluidity. However, the compatibility between inorganic fillers and organic resins is poor. In the present invention, the inorganic filler alumina is modified by coating with dopamine, and the modified inorganic filler can form hydrogen bonds with the carbamate and urea groups of the polyurethane, thereby improving the compatibility of the modified inorganic filler and the polyurethane adhesive.
[0024] 2. The flame retardant and heat-insulating layer prepared by the present invention is obtained by compounding a flame retardant material and aluminum dihydrogen phosphate; dimethyldichlorosilane and ethylenediamine react to obtain an intermediate product A containing the flame retardant element silicon and multiple imino groups and amino groups; the intermediate product A and cyanuric chloride undergo multi-stage nucleophilic substitution to obtain a flame retardant material rich in multiple flame retardant elements of nitrogen and silicon; during the combustion process, an inorganic protective layer containing Si-O or Si-C bonds is formed on the surface of the flame retardant material, thereby slowing down the combustion. The flame retardant material polyimino groups are then reacted with aluminum dihydrogen phosphate having a phosphate group to obtain a flame retardant and heat-insulating material; aluminum dihydrogen phosphate can form a metal oxide aluminum oxide during the combustion process, thereby achieving a flame retardant effect. The present invention performs surface leveling and degreasing pretreatment on the aluminum-zinc-plated substrate to obtain a metal substrate after surface pretreatment, which is convenient for post-processing of the metal substrate; the metal substrate after surface pretreatment is coated with a wear-resistant adhesive and a flame-retardant thermal insulation material to form a wear-resistant adhesive layer and a flame-retardant thermal insulation layer, and then the metal composite plate is dried to prepare a fire-proof and wear-resistant thermal insulation composite plate. DETAILED DESCRIPTION
[0025] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Embodiment 1: This embodiment provides a method for preparing a fire-resistant and wear-resistant thermal insulation composite panel wear-resistant adhesive, comprising the following steps: B1. Weigh 10 g of tris(hydroxymethylaminomethane) powder and 100 mL of deionized water and mix them evenly to obtain a buffer solution of tris(hydroxymethylaminomethane); grind spherical alumina and pass it through a 100-mesh sieve to obtain alumina powder; add 5 g of spherical alumina powder and 0.5 g of dopamine hydrochloride to 100 mL of the buffer solution of tris(hydroxymethylaminomethane), stir at 100 r / min for 24 h, and then filter to obtain a solid material; wash the solid material three times with deionized water, and then dry it in an oven at 60° C. for 24 h to obtain a modified inorganic filler.
[0027] B2. Add 20 g of isophorone diisocyanate, 5 g of 2-mercaptopropionic acid, 60 g of diol and 5 g of modified inorganic filler into a 250 mL three-necked flask, then introduce nitrogen into the three-necked flask as a protective gas, mix and stir at 100 r / min at 70°C for 30 min, then add 0.01 g of catalyst dibutyltin dilaurate, mix and stir at 100 r / min at 70°C, and continue to react for 4 h. After the reaction is completed, a reaction product is obtained; the reaction product is cooled to room temperature, and then 2 g of neutralizing agent triethanolamine is added, and stirring is continued at 1000 r / min for 20 min. 100 mL of deionized water is added dropwise for emulsification to obtain a wear-resistant adhesive.
[0028] Embodiment 2: This embodiment provides a method for preparing a fire-resistant and wear-resistant thermal insulation composite panel wear-resistant adhesive, comprising the following steps: B1. Weigh 12 g of tris(hydroxymethylaminomethane) powder and 100 mL of deionized water and mix them evenly to obtain a buffer solution of tris(hydroxymethylaminomethane); grind spherical alumina and pass it through a 100-mesh sieve to obtain alumina powder; add 8 g of spherical alumina powder and 0.5 g of dopamine hydrochloride to 100 mL of the buffer solution of tris(hydroxymethylaminomethane), stir at 100 r / min for 24 h, and then filter to obtain a solid material; wash the solid material three times with deionized water, and then dry it in an oven at 65° C. for 24 h to obtain a modified inorganic filler.
[0029] B2. Add 25 g of isophorone diisocyanate, 8 g of 2-mercaptopropionic acid, 60 g of diol and 7 g of modified inorganic filler into a 250 mL three-necked flask, then introduce nitrogen into the three-necked flask as a protective gas, mix and stir at 110 r / min at 75 ° C for 30 min, then add 0.01 g of catalyst dibutyltin dilaurate, mix and stir at 110 r / min at 75 ° C, and continue to react for 4.5 h. After the reaction is completed, a reaction product is obtained; the reaction product is cooled to room temperature, and then 3 g of neutralizing agent triethanolamine is added, and stirring is continued at 1000 r / min for 25 min. 100 mL of deionized water is added dropwise for emulsification to obtain a wear-resistant adhesive.
[0030] Embodiment 3: This embodiment provides a method for preparing a fire-resistant and wear-resistant thermal insulation composite panel wear-resistant adhesive, comprising the following steps: B1. Weigh 15 g of tris(hydroxymethylaminomethane) powder and 100 mL of deionized water and mix them evenly to obtain a buffer solution of tris(hydroxymethylaminomethane); grind the spherical alumina and pass it through a 100-mesh sieve to obtain alumina powder; add 10 g of the spherical alumina powder and 0.5 g of dopamine hydrochloride to 100 mL of the buffer solution of tris(hydroxymethylaminomethane), stir at 100 r / min for 24 h, and then filter to obtain a solid material; wash the solid material three times with deionized water, and then dry it in an oven at 70°C for 24 h to obtain a modified inorganic filler.
[0031] B2. Add 30 g of isophorone diisocyanate, 10 g of 2-mercaptopropionic acid, 60 g of diol and 10 g of modified inorganic filler into a 250 mL three-necked flask, then introduce nitrogen into the three-necked flask as a protective gas, mix and stir at 80 ° C at 120 r / min for 30 min, then add 0.01 g of catalyst dibutyltin dilaurate, mix and stir at 80 ° C at 120 r / min, and continue to react for 5 h. After the reaction is completed, a reaction product is obtained; the reaction product is cooled to room temperature, and then 5 g of neutralizing agent triethanolamine is added, and stirring is continued at 1000 r / min for 30 min. 100 mL of deionized water is added dropwise for emulsification to obtain a wear-resistant adhesive.
[0032] Embodiment 4: This embodiment provides a method for preparing a flame retardant thermal insulation material for a fireproof and wear-resistant thermal insulation composite panel, comprising the following steps: S1. Add 12 mL of dimethyldichlorosilane, 5 g of ethylenediamine and 250 mL of dioxane into a 500 mL beaker, then transfer the beaker to a water bath, set the water bath temperature to 60 ° C, mix and stir at 100 r / min for 2 hours, then heat to 90 ° C, mix and stir at 100 r / min, and react for 2 hours to obtain intermediate product A.
[0033] S2. Add 15 g of cyanuric chloride to the intermediate product A, react at 0°C for 2 h, then heat to 50°C, mix and react at 100 r / min for 2 h, then heat to 100°C, mix and react at 100 r / min for 2 h to obtain a product; add the product to 100 mL of deionized water, filter and obtain the product; grind and crush the product through a 100-mesh sieve to obtain a flame retardant material.
[0034] S3. Mix 30 mL of phosphoric acid and 10 g of aluminum hydroxide, and stir at 100 r / min for 30 min to obtain a dihydrogen aluminum phosphate solution; mix the flame retardant material and the dihydrogen aluminum phosphate solution evenly, and then filter to obtain a solid, and vacuum dry the solid at 60° C. for 30 min to obtain a flame retardant thermal insulation material.
[0035] Embodiment 5: This embodiment provides a method for preparing a flame retardant thermal insulation material for a fireproof and wear-resistant thermal insulation composite panel, comprising the following steps: S1. Add 13 mL of dimethyldichlorosilane, 8 g of ethylenediamine and 250 mL of dioxane into a 500 mL beaker, then transfer the beaker to a water bath, set the water bath temperature to 65 ° C, mix and stir at 100 r / min for 2 hours, then heat to 90 ° C, mix and stir at 130 r / min, and react for 2 hours to obtain intermediate product A.
[0036] S2. Add 18g of cyanuric chloride to the intermediate product A, react at 0°C for 2.5h, then heat to 50°C, mix and react at 150r / min for 2.5h, then heat to 100°C, mix and react at 150r / min for 2.5h to obtain a product. Add the product to 100mL of deionized water, filter and obtain the product; grind and crush the product to pass through a 100-mesh sieve to obtain a flame retardant material.
[0037] S3. Mix 30 mL of phosphoric acid and 12 g of aluminum hydroxide, stir at 100 r / min for 30 min to obtain an aluminum dihydrogen phosphate solution; mix the flame retardant material and the aluminum dihydrogen phosphate solution evenly, filter to obtain a solid, and vacuum dry the solid at 66° C. for 30 min to obtain a flame retardant thermal insulation material.
[0038] Embodiment 6: This embodiment provides a method for preparing a flame retardant thermal insulation material for a fireproof and wear-resistant thermal insulation composite panel, comprising the following steps: S1. Add 15 mL of dimethyldichlorosilane, 10 g of ethylenediamine and 250 mL of dioxane into a 500 mL beaker, then transfer the beaker to a water bath, set the water bath temperature to 70 ° C, mix and stir at 100 r / min for 2 h, then heat to 90 ° C, mix and stir at 200 r / min, and react for 2 h to obtain intermediate product A.
[0039] S2. Add 20g of cyanuric chloride to the intermediate product A, react at 0°C for 3h, then heat to 50°C, mix and react at 200r / min for 3h, then heat to 100°C, mix and react at 200r / min for 3h to obtain a product. Add the product to 100mL of deionized water, filter and obtain the product; grind and crush the product to pass through a 100-mesh sieve to obtain a flame retardant material.
[0040] S3. Mix 30 mL of phosphoric acid and 15 g of aluminum hydroxide, and stir at 100 r / min for 30 min to obtain an aluminum dihydrogen phosphate solution; mix the flame retardant material and the aluminum dihydrogen phosphate solution evenly, and then filter to obtain a solid, and vacuum dry the solid at 70° C. for 30 min to obtain a flame retardant thermal insulation material.
[0041] Embodiment 7: This embodiment provides a method for preparing a fireproof and wear-resistant thermal insulation composite board, comprising the following steps: A1. Select an aluminum-zinc-plated substrate with a specification of 0.4×1000mm as a metal substrate, use quartz sand as an abrasive, and grind the surface of the metal substrate at a speed of 10m / s for 5min to obtain a polished metal substrate; use ultrasonic cleaning of the polished metal substrate, use a degreasing agent as a cleaning liquid, the frequency of ultrasonic cleaning is 16kHz, and the duration of ultrasonic cleaning is 10min to obtain a pretreated metal substrate.
[0042] A2. One side of the pretreated metal substrate A is coated with the wear-resistant adhesive prepared in Example 1, and the coating thickness is 10 μm to obtain a first wear-resistant layer; the surface of the first wear-resistant layer is paved with the flame-retardant thermal insulation material prepared in Example 4 to obtain a flame-retardant thermal insulation layer, and the coating thickness is 10 μm; the flame-retardant thermal insulation layer is then coated with the wear-resistant adhesive prepared in Example 1, and the coating thickness is 10 μm to obtain a second wear-resistant layer; then the pretreated metal substrate B is placed to obtain a metal composite plate; the metal composite plate is dried at room temperature for 24 hours, and then dried in a vacuum environment at 70°C for 24 hours, and then the pretreated metal substrate A and the pretreated metal substrate B are brazed to obtain a fire-resistant and wear-resistant thermal insulation composite plate.
[0043] Embodiment 8: This embodiment provides a method for preparing a fireproof and wear-resistant thermal insulation composite board, comprising the following steps: A1. Select an aluminum-zinc-coated substrate with a specification of 0.4×1000mm as a metal substrate, use quartz sand as an abrasive, and grind the surface of the metal substrate at a speed of 10m / s for 6min to obtain a polished metal substrate; use ultrasonic cleaning of the polished metal substrate, use a degreasing agent as a cleaning liquid, the frequency of ultrasonic cleaning is 18kHz, and the duration of ultrasonic cleaning is 15min to obtain a pretreated metal substrate.
[0044] A2. One side of the pretreated metal substrate A is coated with the wear-resistant adhesive prepared in Example 2, and the coating thickness is 15μm to obtain a first wear-resistant layer; the surface of the first wear-resistant layer is paved with the flame-retardant thermal insulation material prepared in Example 5 to obtain a flame-retardant thermal insulation layer, and the coating thickness is 15μm; the flame-retardant thermal insulation layer is then coated with the wear-resistant adhesive prepared in Example 2, and the coating thickness is 15μm to obtain a second wear-resistant layer; then the pretreated metal substrate B is placed to obtain a metal composite plate; the metal composite plate is dried at room temperature for 24h, and then dried in a vacuum environment at 73°C for 24h, and then the pretreated metal substrate A and the pretreated metal substrate B are brazed to obtain a fire-resistant and wear-resistant thermal insulation composite plate.
[0045] Embodiment 9: This embodiment provides a method for preparing a fireproof and wear-resistant thermal insulation composite board, comprising the following steps: A1. Select an aluminum-zinc-coated substrate with a specification of 0.4×1000mm, use quartz sand as an abrasive for the grinding wheel, and grind the surface of the metal substrate with the grinding wheel at a speed of 10m / s for 10min to obtain a polished metal substrate; use ultrasonic cleaning of the polished metal substrate, use a degreasing agent as a cleaning liquid, the frequency of ultrasonic cleaning is 20kHz, and the duration of ultrasonic cleaning is 20min to obtain a pretreated metal substrate.
[0046] A2. Coat one side of the pretreated metal substrate A with the wear-resistant adhesive prepared in Example 3, with a coating thickness of 20 μm, to obtain a first wear-resistant layer; then, lay the flame-retardant thermal insulation material prepared in Example 6 on the surface of the first wear-resistant layer to obtain a flame-retardant thermal insulation layer, with a coating thickness of 20 μm; then, coat the flame-retardant thermal insulation layer with the repair wear-resistant adhesive prepared in Example 3, with a coating thickness of 20 μm, to obtain a second wear-resistant layer; then, place the pretreated metal substrate B to obtain a metal composite plate; dry the metal composite plate at room temperature for 24 hours, then dry it in a vacuum environment at 80°C for 24 hours, and then braze the pretreated metal substrate A and the pretreated metal substrate B to obtain a fire-resistant and wear-resistant thermal insulation composite plate.
[0047] Comparative Example 1: The difference between this comparative example and Example 9 is that step 1 is eliminated and no modified inorganic filler is added in step 2.
[0048] Comparative Example 2: The difference between this comparative example and Example 9 is that 2-mercaptopropionic acid is not added in step 2.
[0049] Comparative Example 3: The difference between this comparative example and Example 9 is that, when preparing the flame retardant thermal insulation material in step 2, the flame retardant material is not modified by using aluminum dihydrogen phosphate solution.
[0050] Performance Test: 1. According to GB7124-2008 "Test of tensile shear strength of adhesives (rigid material to rigid material)", the shear strength of the self-healing polyurethane adhesives prepared in Examples 1-3 and Comparative Example 1 was tested. The test samples were tested using an electronic universal material testing machine with a load capacity of 30KN.
[0051] 2. Perform dynamic mechanical tests on the self-repairing polyurethane adhesives prepared in Examples 1-3 and Comparative Example 1, and record the storage modulus data at 25°C.
[0052] The test results are shown in Table 1: Table 1 Category Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Tensile shear strength / (MPa) 5.5 5.8 6.3 5.1 6.1 Storage modulus / (%) 210.1 213.2 224.5 202.3 180.3 Data Analysis: The polyurethane adhesives prepared in Examples 1-3 of the present invention all have excellent tensile shear strength values and storage modulus values. Since no modified inorganic filler is added when preparing the polyurethane adhesive in Comparative Example 1, the mechanical properties of the prepared adhesive are reduced, which is specifically manifested as a reduction in the tensile shear strength value; in Comparative Example 2, no 2-mercaptopropionic acid is added when preparing the self-repairing polyurethane adhesive, and no thiol group is formed in the polyurethane adhesive, which loses the self-repairing ability, thereby limiting the dynamic reversibility of the polyurethane adhesive, which is manifested as a reduction in the storage modulus value. The reduction in the storage modulus value further depletes the wear resistance of the polyurethane adhesive.
[0053] 3. The fireproof and wear-resistant thermal insulation composite panels prepared in Examples 7-9 and Comparative Example 3 were tested for thermal conductivity using a thermal conductivity tester.
[0054] 4. The total heat release data of the fireproof and wear-resistant thermal insulation composite panels prepared in Examples 7-9 and Comparative Example 3 were recorded using a cone calorimeter.
[0055] The test results are shown in Table 2: Table 2 Category Example 7 Example 8 Example 9 Comparative Example 3 Thermal conductivity / (W / m·k) 0.08 0.06 0.05 5.1 <![CDATA[Total heat release value / (MJ / m 2 )]]> 7.8 8.2 8.5 7.2 Data Analysis: The fireproof and wear-resistant thermal insulation composite panels prepared in Examples 7-9 of the present invention all have excellent thermal insulation properties, which are manifested by low thermal conductivity coefficient values. However, when preparing the flame-retardant thermal insulation material in Comparative Example 3, aluminum dihydrogen phosphate was not used for modification; the thermal conductivity of aluminum dihydrogen phosphate itself is low, which helps to improve the thermal insulation properties of the prepared fireproof and wear-resistant thermal insulation composite panels. In addition, aluminum dihydrogen phosphate itself has a certain flame retardant effect, thereby reducing the total heat release value and further improving the fire resistance of the prepared composite panel.
[0056] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
[0057] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0058] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A fireproof and wear-resistant thermal insulation composite board, It is characterized in that It includes a pre-treated metal substrate A, a first wear-resistant layer, a flame-retardant and heat-insulating layer, a second wear-resistant layer and a pre-treated metal substrate B which are arranged in sequence from bottom to top; The flame retardant thermal insulation layer is prepared from a flame retardant thermal insulation material; The first wear-resistant layer and the second wear-resistant layer are both prepared from a wear-resistant adhesive; The preparation method of the wear-resistant adhesive is as follows: isophorone diisocyanate, 2-mercaptopropionic acid, diol and modified inorganic filler are mixed, mixed and reacted at 70-80° C. for 30 minutes under a nitrogen atmosphere, and then a catalyst is added, and the reaction is continued at 70-80° C. for 4-5 hours to obtain a reaction product; the reaction product is cooled to room temperature, and then a neutralizer is added, and continuous stirring is performed, and deionized water is added dropwise for emulsification to obtain a wear-resistant adhesive layer.
2. A fireproof and wear-resistant thermal insulation composite panel according to claim 1, It is characterized in that The preparation method of the modified inorganic filler is: The tris(hydroxymethyl)aminomethane) powder and deionized water are mixed evenly to obtain a tris(hydroxymethyl)aminomethane buffer solution; the spherical alumina is passed through a 100-mesh sieve to obtain a spherical alumina powder; the tris(hydroxymethyl)aminomethane buffer solution, the spherical alumina powder and dopamine hydrochloride are mixed and stirred at 100 r / min for 24 hours, and then filtered to obtain a solid material; the solid material is washed with deionized water, and then dried at 60-70° C. for 24 hours to obtain a modified inorganic filler.
3. A fireproof and wear-resistant thermal insulation composite panel according to claim 2, It is characterized in that The dosage ratio of tris(hydroxymethyl)aminomethane powder and deionized water is 10-15 g:100 mL; the dosage ratio of tris(hydroxymethyl)aminomethane buffer solution, spherical alumina powder and dopamine hydrochloride is 5-10 g:0.5 g:100 mL.
4. The fireproof and wear-resistant thermal insulation composite panel according to claim 1, It is characterized in that The diol is any one of ethylene glycol, 1,4-butanediol, 1,2-propylene glycol, methyl propylene glycol and a combination thereof; the catalyst is dibutyltin dilaurate; and the neutralizer is ethylenediamine; the dosage ratio of isophorone diisocyanate, 2-mercaptopropionic acid, diol, modified inorganic filler, catalyst and neutralizer is 20-30g:5-10g:60g:5-10g:0.01g:2-5g; the rotation speed of the mixing reaction is 100-120r / min, and the rotation speed of continuous stirring is 1000r / min.
5. The fireproof and wear-resistant thermal insulation composite panel according to claim 1, It is characterized in that The flame retardant heat-insulating material is prepared by the following steps: S1. Mix dimethyldichlorosilane, ethylenediamine and dioxane, stir at 60-70°C for 2h, then heat to 90°C, mix and react for 2h to obtain intermediate product A; add cyanuric chloride to intermediate product A, react at 0°C for 2-3h, then heat to 50°C, mix and react for 2-3h; then heat to 100°C, continue to react for 2-3h to obtain a product; add the product to deionized water, and filter to obtain the product; The product is ground and crushed, and passed through a 100-mesh sieve to obtain a flame retardant material; S2. Mix phosphoric acid and aluminum hydroxide to obtain aluminum dihydrogen phosphate solution; mix the flame retardant material and the aluminum dihydrogen phosphate solution to react, and then filter to obtain a solid; vacuum dry the solid at 60-70° C. for 30 minutes to obtain a flame retardant thermal insulation material.
6. A fireproof and wear-resistant thermal insulation composite panel according to claim 5, It is characterized in that In step S1, the dosage ratio of dimethyldichlorosilane, ethylenediamine, dioxane, cyanuric chloride and deionized water is 12-15mL:5-10g:250mL:15-20g:100mL; the rotation speed of the mixed reaction is 100-200r / min, and the rotation speed of the continuous reaction is 100-200r / min.
7. The fireproof and wear-resistant thermal insulation composite panel according to claim 5, It is characterized in that In step S2, the dosage ratio of phosphoric acid and aluminum hydroxide is 30mL:10-15g; the rotation speed of the mixing reaction is 100r / min, and the duration of the mixing reaction is 30min; the dosage ratio of the flame retardant material and the dialuminum dihydrogen phosphate solution is 10-20g:10mL.
8. A method for preparing a fireproof and wear-resistant thermal insulation composite board, applicable to a fireproof and wear-resistant thermal insulation composite board as claimed in any one of claims 1 to 7, It is characterized in that The following steps are involved: A1. Grinding the surface of the metal substrate with a grinding wheel at a speed of 10 m / s for 5-10 min to obtain a polished metal substrate; ultrasonically cleaning the polished metal substrate with a degreasing agent as a cleaning liquid, the frequency of ultrasonic cleaning is 15-20 kHz, and the duration of ultrasonic cleaning is 10-20 min to obtain a pretreated metal substrate; A2. Coat one side of the pretreated metal substrate A with a wear-resistant adhesive to obtain a first wear-resistant layer; spread a flame-retardant thermal insulation material on the surface of the first wear-resistant layer to obtain a flame-retardant thermal insulation layer; coat the surface of the flame-retardant thermal insulation layer with a wear-resistant adhesive to obtain a second wear-resistant layer; then place the pretreated metal substrate B to obtain a metal composite plate; dry the metal composite plate at room temperature for 24 hours, then dry it in a vacuum environment of 70-80°C for 24 hours, and then braze the pretreated metal substrate A and the pretreated metal substrate B to obtain a fire-resistant and wear-resistant thermal insulation composite plate.
9. A method for preparing a fireproof and wear-resistant thermal insulation composite panel according to claim 8, It is characterized in that The pretreated metal substrate is an aluminum-zinc-plated substrate; the thickness of the first wear-resistant adhesive layer and the second wear-resistant adhesive layer are both 10-20 μm, and the thickness of the flame-retardant thermal insulation layer is 10-20 μm.
Citation Information
Patent Citations
Preparation method of solventless polyurethane adhesive
CN109988538A
High-heat-insulation-property heat preservation composite board and production process thereof
CN114940005A
Recyclable high-strength scratch-resistant self-repairing transparent polyurethane film and preparation method thereof
CN115260446A
Polyurethane adhesive containing polydopamine modified aluminum oxide and preparation method thereof
CN115678480A