Preparation method of copper selenide micro-nano particles

By coating nanoselenium particles on copper substrate and heating treatment, copper selenide micro-nanoparticles are prepared by using integrated coating-evaporation-reaction technology, the problems of complex processes and long time in the existing technology are solved, and multiple sizes are achieved The preparation of copper selenide particles required reduces production costs and time and meets industrial needs.

CN119038497AActive Publication Date: 2024-11-29JIANGXI COPPER CORP +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411238005.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-29
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

The prior art has complex processes, long time, and it is difficult to finely control the particle size when preparing copper selenide micro-nanoparticles, and cannot meet the needs of low-cost, large-scale, and industrialized preparation.

Method used

By configuring the nanoselenium particle solution and applying it uniformly on the surface of the copper substrate, heat treatment is carried out, and the reaction conversion between selenium and copper and powder drying is achieved using the integrated coating-evaporation-reaction technology, and the copper selenide micro-selected on the surface of the copper substrate is collected. Nanoparticles.

Benefits of technology

The process flow is simplified, the preparation time is shortened, and the nano and micro-scale copper selenide micro-nanoparticles can be prepared simultaneously, reducing the time and economic costs of industrial production, and the raw materials and solvents are cheap, which is in line with the policy of green and sustainable development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038497A_ABST
    Figure CN119038497A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of powder metallurgy, in particular to a preparation method of copper selenide micro-nano particles. The method specifically comprises the following steps that ultramicro nano-selenium particle suspension liquid is prepared according to design, the surface of a bright copper substrate is evenly coated with the ultramicro nano-selenium particle suspension liquid in a spin coating mode or a blade coating mode or other modes, the copper substrate is heated at first, after the copper substrate is cooled, powder is collected, and the copper selenide micro-nano particles are obtained. Through rapid chemical reaction of the copper matrix and the ultra-micro nano-selenium particles in the micro-nano scale, the size of the copper selenide powder is uniformly kept in the micro-nano scale, meanwhile, the preparation process of the copper selenide nano-particles is greatly simplified, the copper selenide ultra-micro nano-particles can be prepared in one step, and the preparation process is simple. And the preparation time of the copper selenide ultra-micro nano particles is further shortened. The preparation method has the advantages of easily available raw materials, low cost, simple process, adjustable particle size, efficient and safe flow and extremely high preparation speed, and is very suitable for being used in industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of powder metallurgy, and in particular to a method for preparing copper selenide micro-nano particles. Background Art

[0002] With the gradual development of the energy industry, the development and utilization of new energy sources such as solar energy and wind energy have made great progress. Metal selenides have shown great application potential in optoelectronics, catalysis, new energy and sensors with their excellent performance, and have attracted widespread attention. Among them, copper selenide is a semiconductor with p-type conductivity, and has potential applications in solar cells, filters and superionic materials. At the same time, the micro-nano copper selenide particles not only have the band gap characteristics of large particles themselves, but also have the advantages of nanomaterials. Copper selenide particles at the micro-nano scale have higher comparative area and activity, which can effectively improve the catalytic effect in the catalytic process; at the same time, studies have shown that copper selenide of different particle sizes may have different energy band gaps, which further enhances the application field and potential of copper selenide.

[0003] In the current study, Huang Hong et al. (authorization announcement number CN115347174A) prepared copper selenide porous octahedrons with a diameter of 2 to 3 μm by calcining Cu-MOF and selenium powder in a protective atmosphere for 2 to 8 hours, thereby improving the rate performance of sodium ion batteries; He Ping et al. (authorization announcement number CN115025748A) obtained large flaky copper selenide particles by dissolving selenium powder in sodium hydroxide, adding copper sulfate solution and heating and aging for 24 hours, washing with water and ethanol several times, and drying at 60°C for 12 hours; Liang Changhao et al. (authorization announcement number CN114590832A) obtained non-stoichiometric nano copper selenide by laser irradiating the selenium solution, adding copper foil to the solution for reaction for 24 to 72 hours, and then centrifugally drying.

[0004] Through the above search, it can be found that the current technology is mainly through thermal decomposition of precursors, solvent thermal synthesis, and laser irradiation, which not only requires a more complicated process flow, but the overall preparation time usually ranges from several hours to dozens of hours, and the powder needs to go through a long drying process; in addition, it is difficult to simultaneously finely control the particle size of copper selenide powder to nanometer or micron level under the same process. Therefore, for commercial copper selenide micro-nanoparticles with a wide range of particle size requirements, current technology is difficult to meet the production line requirements of low-cost, large-scale, industrialized preparation. Summary of the invention

[0005] The invention discloses a method for preparing copper selenide micro-nano particles to solve any of the above and other potential problems in the prior art.

[0006] In order to solve the above technical problems, the technical solution of the present invention is: a method for preparing copper selenide micro-nano particles, the preparation method specifically comprising the following steps:

[0007] S1) preparing a nano-selenium particle solution;

[0008] S2) uniformly coating the nano-selenium particle solution obtained in S1) on the surface of the copper substrate;

[0009] S3) heating the copper substrate coated with the selenium particle suspension obtained in S2), keeping the temperature for a period of time, cooling to room temperature, and collecting the powder on the surface of the copper substrate to obtain copper selenide micro-nano particles.

[0010] Further, the specific steps of S1) are:

[0011] S1.1) firstly mix the selenium particles and the solvent in a mass ratio of 1:10 to 1:100 to obtain a mixed solution;

[0012] S1.2) The mixed solution obtained in S1.1) is subjected to ultrasonic stirring to obtain a nano-selenium particle solution.

[0013] Furthermore, the particle size of the selenium particles in S1.1) is 1 to 1000 nm or 1 to 1000 μm; and the solvent is an inorganic solvent or an organic solvent.

[0014] Furthermore, the specific process parameters of the ultrasonic stirring in S1.2) are: a stirring speed of 50 to 500 rpm and an ultrasonic power of 5 to 20 kW.

[0015] Furthermore, the solvent includes an organic solvent and an inorganic solvent; the inorganic solvent includes pure water and ultrapure water; the organic solvent includes methanol, ethanol, propanol, acetone, dimethylamide and toluene.

[0016] Furthermore, the coating method in S2) includes spin coating and scraper coating; the coating thickness is 10 μm to 1 cm.

[0017] Furthermore, the surface of the copper substrate in S2) should be cleaned before coating, and the cleansing pretreatment can be carried out in various ways such as grinding and polishing, pickling, and ultrasonic cleaning.

[0018] Furthermore, the heating temperature in S3) is the boiling point temperature of the solvent of the nano-selenium particle solution ±20 degrees, and the insulation time is 5 to 10 minutes.

[0019] Furthermore, the heating method in S3) includes resistive heating and inductive heating.

[0020] Furthermore, the particle size of the copper selenide micro-nano particles is 1 nm to 1000 μm.

[0021] A copper selenide micro-nano particle is prepared by adopting the above-mentioned preparation method.

[0022] The beneficial effects of the present invention are:

[0023] 1. The method of the present invention overcomes the potential safety hazard of the existing solvent thermal high-pressure reaction of copper selenide particles, and prepares copper selenide micro-nano particles through normal pressure reaction throughout the process. The process is simple and is conducive to large-scale commercial production.

[0024] 2. The method described in the present invention can be simultaneously applied to the preparation of nano- and micron-sized copper selenide micro-nano particles, and even millimeter- or centimeter-sized copper selenide large particles, and has the characteristics of meeting multiple size requirements in one, thereby reducing the construction demand and construction cost of the industrial copper selenide multi-scale particle industry chain.

[0025] 3. The method described in the present invention makes up for the shortcomings of the existing synthesis technology, which is time-consuming and has many steps. By utilizing the coating-evaporation-reaction integrated technology, the reaction conversion of selenium and copper, powder drying and other processes can be realized simultaneously. The preparation of copper selenide micro-nano particles and powder collection can be realized within 5 to 10 minutes, which is time-saving and can effectively reduce the time and economic cost of large-scale industrialization.

[0026] 4. The method described in the present invention has low-priced raw materials and solvents and a wide range of sources, which greatly reduces the preparation cost of copper selenide micro-nano particles. The preparation process is environmentally friendly and complies with the national policy of green and sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The present invention is a flowchart of an ultrafast preparation method of copper selenide micro-nano particles.

[0028] Figure 2 The morphology and elemental energy spectrum distribution diagram of the copper selenide nanoparticles prepared in Example 1 of the present invention.

[0029] Figure 3 This is a size distribution diagram of copper selenide nanoparticles prepared in Example 1 of the present invention.

[0030] Figure 4 This is the morphology and size distribution diagram of the copper selenide micron particles prepared in Example 2 of the present invention.

[0031] Figure 5 This is the morphology and size distribution diagram of copper selenide micron particles prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0032] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.

[0033] like Figure 1As shown, the present invention provides an ultrafast preparation method of copper selenide micro-nano particles, characterized in that the method specifically comprises the following steps:

[0034] S1) preparing a nano-selenium particle solution;

[0035] The specific steps are:

[0036] S1.1) firstly mix the selenium particles and the solvent in a mass ratio of 1:10 to 1:100 to obtain a mixed solution;

[0037] S1.2) The mixed solution obtained in S1.1) is subjected to ultrasonic stirring to obtain a nano-selenium particle solution.

[0038] S2) uniformly coating the nano-selenium particle solution obtained in S1) on the surface of the copper substrate;

[0039] S3) heating the copper substrate coated with the selenium particle suspension obtained in S2), keeping the temperature for a period of time, cooling to room temperature, and collecting the powder on the surface of the copper substrate to obtain copper selenide micro-nano particles.

[0040] The size of the selenium particles in S1) may be 1 to 1000 nm or 1 to 1000 μm;

[0041] The ratio of selenium particles to solvent in S1) is 1:10 to 1:100 by mass;

[0042] The solvent in S1) may be an inorganic solvent such as pure water or ultrapure water, or an organic solvent such as methanol, ethanol, propanol, acetone, dimethylformamide, toluene, etc.

[0043] In said S1), the stirring speed is 50-500 rpm and the ultrasonic power is 5-20 kW;

[0044] The coating method of S2) can be various coating methods such as spin coating and scraping coating;

[0045] The coating thickness of S2) is in the range of 10 μm to 1 cm;

[0046] The surface of the copper substrate in S2) should be cleaned and pre-treated to ensure sufficient contact between the nano-selenium particles and the copper substrate;

[0047] The copper substrate heating method of S3) can be resistive or inductive;

[0048] The heating temperature of the copper substrate in S3) should be controlled within the boiling point of the solvent of the nano-selenium particle solution ±20 degrees to increase the preparation speed of the ultrafine selenide copper nanopowder;

[0049] The copper substrate heating time of S3) is about 5 to 10 minutes;

[0050] The final cooling temperature of the copper substrate in S3) can be controlled at 25-50° C. according to the actual production speed requirements;

[0051] The particle size of the copper selenide micro-nano particles can be controlled within the range of 1 nm to 1000 μm.

[0052] Example 1

[0053] (1) Preparation of nano-selenium suspension solution: Nano-selenium particles with a size range of 1 to 500 nm are added to ethanol, with the ratio of nano-selenium particles to ethanol being 1:50 (mass ratio), and then stirred at a speed of 200 rpm for 3 minutes, and then ultrasonicated in an ultrasonic cleaning machine with an ultrasonic power of 10 kW and an ultrasonic time of 2 minutes to obtain a uniformly mixed nano-selenium suspension solution.

[0054] (2) Preparation of copper selenide nanoparticles: The nano-selenium suspension solution obtained in the previous step is evenly coated on the surface of the copper substrate after acid washing and cleaning pretreatment by spin coating, with a coating thickness of 50 μm. The temperature of the copper substrate is then rapidly raised to 70° C. by resistance heating. After heating for 5 minutes, the powder on the surface of the copper substrate is collected to obtain copper selenide nanoparticles.

[0055] (3) The copper selenide nanoparticles prepared in the example have a D50 of 352 nm and a spherical shape. The test results are shown in the attached figure. Figure 2 and 3 shown.

[0056] Example 2

[0057] (1) Preparation of micron selenium suspension solution: micron selenium particles with a size range of 1 to 10 μm are added to water, with the ratio of micron selenium particles to water being 1:90 (mass ratio), and then stirred at a speed of 450 rpm for 5 minutes, and then ultrasonicated in an ultrasonic cleaning machine with an ultrasonic power of 15 kW and an ultrasonic time of 2 minutes to obtain a uniformly mixed micron selenium suspension solution.

[0058] (2) Preparation of copper selenide nanoparticles: The micron selenium suspension solution obtained in the previous step is evenly coated on the surface of the copper substrate after ultrasonic cleaning and pretreatment by scraping, with a coating thickness of 100 μm. Then, the temperature of the copper substrate is rapidly raised to 105° C. by inductive heating. After heating for 9 minutes, the powder on the surface of the copper substrate is collected to obtain copper selenide microparticles.

[0059] (3) The D50 of the copper selenide microparticles prepared in the example is 3.885 μm, and the morphology is mainly spherical. The test results are shown in the attached figure. Figure 4 shown.

[0060] The above is an embodiment of the present invention with better effects, which is non-limiting to the present invention and is only used to illustrate the detailed preparation process of the present invention, but does not mean that the present invention is limited to the above preparation process. It should be noted that any simple improvement and content modification of the technology of the present invention, without departing from the technical scope of the present invention, belongs to the protection scope of the technical solution of the present invention.

[0061] Comparative Example 1

[0062] (1) Preparation of nano-selenium suspension solution: Nano-selenium particles with a size range of 1 to 500 nm are added to ethanol, with the ratio of nano-selenium particles to ethanol being 1:5 (mass ratio), and then stirred at a speed of 10 rpm for 1 minute, and then ultrasonicated in an ultrasonic cleaning machine with an ultrasonic power of 10 kW and an ultrasonic time of 2 minutes to obtain a nano-selenium suspension solution.

[0063] (2) Preparation of copper selenide nanoparticles: The nano-selenium suspension solution obtained in the previous step was evenly coated on the surface of the copper substrate after acid washing and cleaning pretreatment by scraping, with a coating thickness of 1 cm. Then, the temperature of the copper substrate was rapidly raised to 70°C by resistance heating. After heating for 20 minutes, the powder on the surface of the copper substrate was collected.

[0064] (3) The D50 of the copper selenide particles prepared in the example is 4.442 μm, which does not meet the nanoscale requirement of particle size <1 μm. The test results are shown in the attached figure. Figure 5 shown.

[0065] The above is a detailed introduction to the preparation method of copper selenide micro-nanoparticles provided in the embodiment of the present application. The description of the above embodiment is only used to help understand the method and core idea of ​​the present application; at the same time, for those skilled in the art, according to the idea of ​​the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as limiting the present application.

[0066] For example, certain words are used in the specification and claims to refer to specific components. Those skilled in the art should understand that hardware manufacturers may use different nouns to refer to the same component. This specification and claims do not use differences in names as a way to distinguish components, but use differences in the functions of components as the criteria for distinction. As mentioned throughout the specification and claims, "including" and "comprising" are open-ended terms, so they should be interpreted as "including / including but not limited to". "Approximately" means that within an acceptable error range, those skilled in the art can solve the technical problem within a certain error range and basically achieve the technical effect. The subsequent description of the specification is a preferred embodiment of the present application, but the description is for the purpose of illustrating the general principles of the present application, and is not used to limit the scope of the present application. The scope of protection of the present application shall be determined by the definition of the attached claims.

[0067] It should also be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a product or system including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such a product or system. In the absence of more restrictions, the elements defined by the sentence "comprises a ..." do not exclude the existence of other identical elements in the product or system including the elements.

[0068] It should be understood that the term "and / or" used in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0069] The above description shows and describes several preferred embodiments of the present application, but as mentioned above, it should be understood that the present application is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the application concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art do not deviate from the spirit and scope of the present application, and should be within the scope of protection of the claims attached to the present application.

Claims

1. A method for preparing copper selenide micro-nano particles, characterized in that: The preparation method specifically comprises the following steps: S1) preparing a nano-selenium particle solution; S2) uniformly coating the nano-selenium particle solution obtained in S1) on the surface of the copper substrate; S3) heating the copper substrate coated with the selenium particle suspension obtained in S2), keeping the temperature for a period of time, cooling to room temperature, and collecting the powder on the surface of the copper substrate to obtain copper selenide micro-nano particles.

2. The preparation method according to claim 1, characterized in that: The specific steps of S1) are: S1.1) firstly mix the selenium particles and the solvent in a mass ratio of 1:10 to 1:100 to obtain a mixed solution; S1.2) The mixed solution obtained in S1.1) is subjected to ultrasonic stirring to obtain a nano-selenium particle solution.

3. The preparation method according to claim 2, characterized in that: The particle size of the selenium particles in S1.1) is 1 to 1000 nm or 1 to 1000 μm; the solvent is an inorganic solvent or an organic solvent.

4. The preparation method according to claim 2, characterized in that: The specific process parameters of the ultrasonic stirring in S1.2) are: stirring speed of 50-500 rpm, and ultrasonic power of 5-20 kW.

5. The preparation method according to claim 2, characterized in that: The solvent includes an organic solvent and an inorganic solvent; the inorganic solvent includes pure water and ultrapure water; the organic solvent includes methanol, ethanol, propanol, acetone, dimethylamide and toluene.

6. The preparation method according to claim 1, characterized in that: The coating method in S2) includes spin coating and scraping coating; the coating thickness is 10 μm to 1 cm.

7. The preparation method according to claim 1, characterized in that: The heating temperature in S3) is the boiling point temperature of the solvent of the nano-selenium particle solution ± 20 degrees, and the insulation time is 5 to 10 minutes.

8. The preparation method according to claim 1, characterized in that: The heating methods in S3) include resistive and inductive heating.

9. The preparation method according to claim 1, characterized in that: The particle size of the copper selenide micro-nano particles is 1 nm to 1000 μm.

10. A copper selenide micro-nano particle, characterized in that: The copper selenide micro-nano particles are prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Copper selenide fluorescent quantum dot and preparation method and application thereof

    CN103803511A

  • Preparation method and application of copper selenide nanosheet array for sodium ion battery with adjustable interlayer spacing

    CN110371936A

  • Compound Semiconductors and their manufacturing method

    KR1020150137741A

  • Method for producing a polarisation-sensitive nanocomposite film based on copper selenide

    RU2758150C1

  • Liquid precursor for deposition of copper selenide and method of preparing the same

    US20110312160A1