Preparation method of high-capacity hard carbon negative electrode material, negative electrode plate and battery

By mixing the carbon source with the porous material and carbonized in an inert atmosphere, a hard carbon material containing closed pores was prepared, which solved the problem of insufficient specific capacity and Coulomb efficiency in sodium ion batteries, and achieved high A hard carbon anode material for sodium ion battery with capacity and high efficiency, and this method is simple and environmentally friendly, suitable for large-scale production.

CN119038516APending Publication Date: 2024-11-29JIANGSU HUAHONG SODIUM TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410610097.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-16
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The application of existing hard carbon materials in sodium ion batteries is limited by the adsorption-embedding-hole filling mechanism, which makes the actual specific capacity difficult to satisfy. Commonly used improved methods such as heteroatom doping and making openings will reduce the first Coulomb efficiency. Moreover, the processing steps of the hard template method are cumbersome and may lead to environmental pollution.

Method used

By mixing the carbon source with the porous material and carbonized in an inert atmosphere, a hard carbon material containing closed pores is prepared, and a combination of a carbon source such as cellulose, sucrose, etc. and a porous material such as ZIF-8, KB, etc. is used to perform carbonization. Processing to improve the specific capacity of hard carbon and first-time Coulomb efficiency.

Benefits of technology

The specific capacity of hard carbon negative electrode materials has been significantly improved and the first Coulomb efficiency has been improved. At the same time, the method is simple, environmentally friendly, low-cost, and suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of batteries, and particularly relates to a preparation method of a high-capacity hard carbon negative electrode material, a negative electrode plate and a battery. The preparation method comprises the following steps: S1, fully mixing a carbon source and a porous material, and drying to obtain a precursor; and S2, carrying out carbonization treatment on the precursor obtained in the step S1 at 1000-1800 DEG C in an inert atmosphere, carrying out heat preservation for 2-15 hours, and then cooling to obtain the sodium-ion battery hard carbon negative electrode material. The invention also provides the battery hard carbon negative electrode material prepared by the method, and a negative plate and a battery made of the material. According to the preparation method of the sodium ion battery hard carbon negative electrode material provided by the invention, the specific capacity and the first coulombic efficiency of the hard carbon negative electrode material can be remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of batteries, and specifically relates to a method for preparing a high-capacity hard carbon negative electrode material, a negative electrode sheet and a battery. Background Art

[0002] In order to solve problems such as energy and environmental crises, the development and utilization of renewable resources have received increasing attention. Lithium-ion batteries have been widely used in commercial portable electronic devices, energy storage, and electric / hybrid vehicles. However, with the increasing demand for energy storage devices such as portable electronic devices and electric / hybrid vehicles, the amount of lithium required for the growth of lithium-ion batteries is expected to be unable to be provided by existing resources in the near future. Therefore, there is an urgent need to research and develop a new generation of secondary battery energy storage technology with excellent performance.

[0003] Considering the low cost of sodium resources, the advantages of abundant reserves, and similar properties to lithium, sodium-ion batteries are regarded as one of the most promising alternatives to lithium-ion batteries. However, due to their narrow carbon interlayer spacing and thermodynamic instability of intercalation compounds, the application of traditional graphite negative electrode materials in sodium-ion batteries has not met expectations. Therefore, graphite is not suitable for anode materials of sodium-ion batteries. Hard carbon, as another carbon-based material, has a larger interlayer gap than graphite, which can meet the needs of sodium ion insertion / extraction and can provide higher reversible capacity. Therefore, hard carbon is considered to be one of the most promising anode materials for sodium-ion batteries.

[0004] However, current hard carbon materials are limited by the adsorption-embedding-pore filling mechanism, and the actual specific capacity they provide is often unsatisfactory. In order to enhance the sodium storage capacity of hard carbon, a variety of methods have been tried. For example, heteroatom doping (1), making pores (2), hard template method pore creation (3-5), etc. However, heteroatom doping and making pores often lead to a significant decrease in the first coulombic efficiency (ICE) and volumetric energy density. At the same time, although the hard template method is an effective means to increase capacity, it is usually accompanied by cumbersome processing steps. In addition, strong acid and strong base solutions may need to be used when processing the template, which may cause environmental pollution and is not conducive to sustainable development. Summary of the invention

[0005] The present invention provides a method for preparing a hard carbon product containing closed pores by carbonizing a porous material and a carbon source together. The hard carbon material finally prepared has a relatively good specific capacity and an excellent first coulombic efficiency.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A method for preparing a hard carbon negative electrode material for a sodium ion battery comprises the following steps:

[0008] S1: fully mix the carbon source and the porous material, and obtain a precursor after drying;

[0009] S2: The precursor obtained in step S1 is carbonized at 1000° C. to 1800° C. in an inert atmosphere for 2 to 15 hours, and then cooled to obtain a hard carbon negative electrode material for a sodium ion battery.

[0010] Furthermore, the carbon source in step S1 includes one or more combinations of cellulose, sucrose, xylose, fructose, glucose, epoxy resin, phenolic resin, polyethylene, and polypropylene.

[0011] Furthermore, the porous material in step S1 includes one or more combinations of ZIF-8, KB, activated carbon, graphene, and carbon nanotubes.

[0012] Furthermore, in step S1, the carbon source and the porous material are fully mixed by stirring, mechanical ball milling, mechanical crushing or mechanical compression.

[0013] Furthermore, the inert atmosphere in step S2 is any one of argon, helium, nitrogen, and a hydrogen-argon mixture.

[0014] Furthermore, the heating rate of the carbonization treatment in step S2 is 1-5°C / min.

[0015] The present invention also provides a sodium ion battery hard carbon negative electrode material, and the sodium ion battery hard carbon negative electrode material is prepared by the preparation method of the sodium ion battery hard carbon negative electrode material.

[0016] The present invention also provides a negative electrode sheet for a sodium ion battery, comprising the above-mentioned hard carbon negative electrode material for a sodium ion battery.

[0017] The present invention also provides a sodium ion battery, comprising the negative electrode sheet for the sodium ion battery.

[0018] Beneficial effects of the present invention:

[0019] (1) The method for preparing the hard carbon negative electrode material proposed in the present invention has the advantages of being simple, environmentally friendly, and low-cost, and is suitable for large-scale production.

[0020] (2) The preparation method of the hard carbon negative electrode material for sodium ion batteries provided by the present invention can significantly improve the specific capacity and first coulombic efficiency of the hard carbon negative electrode material. DETAILED DESCRIPTION

[0021] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] Preferably, the above-mentioned feature item is a method for preparing a high-capacity hard carbon negative electrode material and its specific implementation scheme is as follows:

[0023] Example 1

[0024] The method for preparing the hard carbon negative electrode material provided in this embodiment comprises the following steps:

[0025] Treatment of precursor materials: 0.25 g of ZIF-8 and 9.75 g of sucrose (ie, the mass ratio of carbon source to porous material is 39:1) were placed in a ball mill, the ball mill speed was 300 rpm, and the ball milling time was 2 h.

[0026] Pyrolysis carbonization: The precursor material obtained above is placed in a tube furnace and carbonized in an argon atmosphere at a carbonization temperature of 1400°C for 3 hours, wherein the tube furnace temperature rise rate is 4°C / min. Then, the argon is continued to be naturally cooled to 25-30°C to obtain a hard carbon negative electrode material.

[0027] The obtained hard carbon was used as the negative electrode material, the sodium sheet as the positive electrode, the electrolyte was 1M NaCF3SO3 in DIGLYMEelectrolyte, and the separator was glass fiber (GF / C) to carry out electrochemical tests. The first discharge specific capacity was 308mAh g-1 at a current density of 30mA g-1, and the first efficiency was 87.5%.

[0028] Example 2

[0029] The method for preparing the hard carbon negative electrode material provided in this embodiment comprises the following steps:

[0030] Treatment of precursor materials: 0.5 g of ZIF-8 and 9.5 g of sucrose (ie, the mass ratio of carbon source to porous material is 19:1) were placed in a ball mill, the ball mill speed was 300 rpm, and the ball milling time was 2 h.

[0031] Pyrolysis carbonization: The precursor material obtained above is placed in a tube furnace and carbonized in an argon atmosphere at a carbonization temperature of 1400°C for 3 hours, wherein the tube furnace temperature rise rate is 4°C / min. Then, the argon is continued to be naturally cooled to 25-30°C to obtain a hard carbon negative electrode material.

[0032] The obtained hard carbon was used as the negative electrode material, the sodium sheet as the positive electrode, the electrolyte was 1M NaCF3SO3 in DIGLYMEelectrolyte, and the separator was glass fiber (GF / C) to carry out electrochemical tests. The first discharge specific capacity was 331mAh g-1 at a current density of 30mA g-1, and the first efficiency was 87.9%.

[0033] Example 3

[0034] 20g NaCl, 20g KCl and 200g starch were ball-milled at 300 rpm for 6 hours. The mixed composite material was placed in a tubular furnace in an Ar atmosphere, heated to 600°C at 1.5°C per minute and kept warm for 1 hour. The sample after the first step of carbonization was soaked in 50mL HCl (2M) solution for 4 hours, rinsed and dried, and placed in a tubular furnace in an N2 atmosphere again, heated to 1350°C at 5°C per minute and kept warm for 3 hours. After cooling, the hard carbon negative electrode material was obtained.

[0035] The first discharge capacity of this hard carbon anode material at a current density of 0.1C is 334.7 mAh g -1 , the initial effect is 90.2%.

[0036] Example 4

[0037] The method for preparing the hard carbon negative electrode material provided in this embodiment comprises the following steps:

[0038] Treatment of precursor materials: 1 g of ZIF-8 and 9 g of sucrose (ie, the mass ratio of carbon source to porous material is 9:1) were placed in a ball mill, the ball mill speed was 300 rpm, and the ball milling time was 2 h.

[0039] Pyrolysis carbonization: The precursor material obtained above is placed in a tube furnace and carbonized in an argon atmosphere at a carbonization temperature of 1400°C for 3 hours, wherein the tube furnace temperature rise rate is 4°C / min. Then, the argon is continued to be naturally cooled to 25-30°C to obtain a hard carbon negative electrode material.

[0040] The obtained hard carbon was used as the negative electrode material, the sodium sheet as the positive electrode, the electrolyte was 1M NaCF3SO3 in DIGLYMEelectrolyte, and the separator was glass fiber (GF / C) to carry out electrochemical tests. The first discharge capacity was 356mAh g-1 at a current density of 30mA g-1, and the first efficiency was 89.5%.

[0041] Example 5

[0042] The method for preparing the hard carbon negative electrode material provided in this embodiment comprises the following steps:

[0043] Treatment of precursor materials: 1.25 g of ZIF-8 and 8.75 g of sucrose (ie, the mass ratio of carbon source to porous material is 7:1) were placed in a ball mill, the ball mill speed was 300 rpm, and the ball milling time was 2 h.

[0044] Pyrolysis carbonization: The precursor material obtained above is placed in a tube furnace and carbonized in an argon atmosphere at a carbonization temperature of 1400°C for 3 hours, wherein the tube furnace temperature rise rate is 4°C / min. Then, the argon is continued to be naturally cooled to 25-30°C to obtain a hard carbon negative electrode material.

[0045] The obtained hard carbon was used as the negative electrode material, the sodium sheet as the positive electrode, the electrolyte was 1M NaCF3SO3 in DIGLYMEelectrolyte, and the separator was glass fiber (GF / C) to carry out electrochemical tests. The first discharge specific capacity was 334mAh g-1 at a current density of 30mA g-1, and the first efficiency was 88.5%.

[0046] Example 6

[0047] The method for preparing the hard carbon negative electrode material provided in this embodiment comprises the following steps:

[0048] Treatment of precursor materials: 1.5 g of ZIF-8 and 8.5 g of sucrose (ie, the mass ratio of carbon source to porous material is 5.67:1) were placed in a ball mill, the ball mill speed was 300 rpm, and the ball milling time was 2 h.

[0049] Pyrolysis carbonization: The precursor material obtained above is placed in a tube furnace and carbonized in an argon atmosphere at a carbonization temperature of 1400°C for 3 hours, wherein the tube furnace temperature rise rate is 4°C / min. Then, the argon is continued to be naturally cooled to 25-30°C to obtain a hard carbon negative electrode material.

[0050] The obtained hard carbon was used as the negative electrode material, the sodium sheet as the positive electrode, the electrolyte was 1M NaCF3SO3 in DIGLYMEelectrolyte, and the separator was glass fiber (GF / C) to carry out electrochemical tests. The first discharge specific capacity was 311mAh g-1 at a current density of 30mA g-1, and the first efficiency was 88.1%.

[0051] Example 7

[0052] The method for preparing the hard carbon negative electrode material provided in this embodiment comprises the following steps:

[0053] Treatment of precursor materials: 1.75 g of activated carbon and 8.25 g of sucrose (ie, the mass ratio of carbon source to porous material is 4.71:1) are placed in a ball mill, the ball mill speed is 300 rpm, and the ball milling time is 2 h.

[0054] Pyrolysis carbonization: The precursor material obtained above is placed in a tube furnace and carbonized in an argon atmosphere at a carbonization temperature of 1400°C for 3 hours, wherein the tube furnace temperature rise rate is 4°C / min. Then, the argon is continued to be naturally cooled to 25-30°C to obtain a hard carbon negative electrode material.

[0055] The obtained hard carbon was used as the negative electrode material, the sodium sheet as the positive electrode, the electrolyte was 1M NaCF3SO3 in DIGLYMEelectrolyte, and the separator was glass fiber (GF / C) to carry out electrochemical tests. The first discharge specific capacity was 310mAh g-1 at a current density of 30mA g-1, and the first efficiency was 87.4%.

[0056] Comparative Example 1

[0057] The preparation method of the hard carbon negative electrode material provided in this comparative example is basically the same as that of Examples 1-7, except that the mixture of sucrose and porous material in the precursor is replaced with pure sucrose of equal mass. The obtained hard carbon is used as the negative electrode material, the sodium sheet is used as the positive electrode, the electrolyte is 1M NaCF3SO3 in DIGLYME electrolyte, and the separator is glass fiber (GF / C) to carry out electrochemical testing. The first discharge specific capacity is 280mAh g-1 at a current density of 30mA g-1, and the first efficiency is 85.2%.

[0058] The first discharge specific capacity and first effect results of Examples 1-7 and Comparative Example 1 at a current density of 30 mA g-1 are shown in the following table: project Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Comparative Example 1 <![CDATA[Initial discharge specific capacity (mAh g -1 )]]> 308 331 332 356 334 311 310 280 First coulombic efficiency (%) 87.5 87.9 88.8 89.5 88.5 88.1 87.4 85.2 Table 1 Comparison of first discharge specific capacity and first coulombic efficiency of Examples 1-7 and Comparative Example 1 By comparing the experimental results of Examples 1 to 7, it can be found that the carbon source and porous material used in the present invention are used as precursors, and a hard carbon product with excellent sodium storage performance is successfully prepared by a method of simple mixing and carbonization. The first discharge specific capacity of the hard carbon negative electrode material at a current density of 30 mA g-1 is greater than 308 mAh g-1, and the first coulomb efficiency is greater than 87.4%. It shows excellent discharge specific capacity and first coulomb efficiency. The preparation method has the advantages of simplicity, environmental protection, and low cost, and is very suitable for large-scale production of hard carbon products.

[0062] Example 8

[0063] This embodiment provides a sodium ion battery hard carbon negative electrode material, which is made by any one of the methods in Embodiments 1-7.

[0064] Example 9

[0065] This embodiment provides a negative electrode sheet for a sodium ion battery, using the sodium ion battery hard carbon negative electrode material provided in Example 8.

[0066] Example 10

[0067] This embodiment provides a sodium ion battery, comprising the negative electrode sheet for sodium ion battery provided in Embodiment 9.

[0068] The above contents are only actual examples of the test objects of the test method of the present invention, and are not intended to limit the implementation scheme of the present invention. A person skilled in the art can easily make corresponding changes or modifications based on the main concept and spirit of the invention of the test method, because the protection scope of the present invention shall be based on the protection scope required by the claims.

Claims

1. A method for preparing a hard carbon negative electrode material for a sodium ion battery, characterized in that: The steps include: S1: fully mix the carbon source and the porous material, and obtain a precursor after drying; S2: The precursor obtained in step S1 is carbonized at 1000° C. to 1800° C. in an inert atmosphere for 2 to 15 hours, and then cooled to obtain a hard carbon negative electrode material for a sodium ion battery.

2. The method for preparing the hard carbon negative electrode material for sodium ion batteries according to claim 1, characterized in that: The carbon source in step S1 includes one or more combinations of cellulose, sucrose, xylose, fructose, glucose, epoxy resin, phenolic resin, polyethylene, and polypropylene.

3. The method for preparing the hard carbon negative electrode material for sodium ion battery according to claim 1, characterized in that: The porous material in step S1 includes one or more combinations of ZIF-8, KB, activated carbon, graphene, and carbon nanotubes.

4. The method for preparing the hard carbon negative electrode material for sodium ion battery according to claim 1, characterized in that: In step S1, the carbon source and the porous material are fully mixed by stirring, mechanical ball milling, mechanical crushing or mechanical compression.

5. The method for preparing the hard carbon negative electrode material for sodium ion batteries according to claim 1, characterized in that: The inert atmosphere in step S2 is any one of argon, helium, nitrogen, and a hydrogen-argon mixture.

6. The method for preparing the hard carbon negative electrode material for sodium ion battery according to claim 1, characterized in that: The heating rate of the carbonization treatment in step S2 is 1-5°C / min.

7. A hard carbon negative electrode material for a sodium ion battery, characterized in that: The sodium ion battery hard carbon negative electrode material is prepared by any method of claims 1-6.

8. A negative electrode sheet for a sodium ion battery, characterized in that: Comprising the sodium ion battery hard carbon negative electrode material as described in claim 7.

9. A sodium ion battery, characterized in that: The negative electrode sheet for a sodium ion battery according to claim 9 is included.

Citation Information

Patent Citations

  • Preparation method and application of carbon material based on co-carbonization of porous carbon and thermoplastic carbon source

    CN114275764A

  • Modified porous carbon material as well as preparation method and application thereof

    CN116062734A

  • Method for preparing hard carbon negative electrode material by using waste thermosetting plastic

    CN116102012A

  • Metal quantum dot / hard carbon negative electrode material and preparation method thereof

    CN116169288A

  • Preparation method of porous carbon