Ni3S4-MoS2 heterojunction material as well as preparation method and application thereof

By using Ni3S4-MoS2 heterojunction material as the transduction layer in all solid state ion selective electrodes, the problem of poor electrode stability and reproducibility is solved, and the combination of high capacitance and hydrophobicity is achieved, which significantly improves the potential response and stability sex.

CN119038636APending Publication Date: 2024-11-29WANJIANG EMERGING IND TECH DEV CENT +2
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411152847.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The poor stability and poor reproducibility of all-solid-state ion selective electrodes in potential response are mainly due to the insufficient capacitance and hydrophobicity of the solid contact layer.

Method used

Ni3S4-MoS2 heterojunction material was prepared by one-step hydrothermal method and used as the transducing layer material for all-solid sodium ion selective electrodes. The electron redistribution and hydrophobicity of MoS2 are improved through the introduction of Ni, and the active site is increased. and specific surface area.

Benefits of technology

The potential response stability and reproducibility of the electrode are significantly improved, the capacitance and hydrophobicity are enhanced, and the good potential response, stability and reversibility are achieved, and the stability of the low-surface water layer on the electrode is maintained in long-term use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038636A_ABST
    Figure CN119038636A_ABST
Patent Text Reader

Abstract

The invention discloses a Ni3S4-MoS2 heterojunction material as well as a preparation method and application thereof, and belongs to the technical field of ion selective electrodes. The preparation method of the Ni3S4-MoS2 heterojunction material comprises the following steps: adding a molybdenum source, a nickel source and a sulfur source into water, and performing ultrasonic dispersion to form a uniform mixed solution; the mixed solution is subjected to a hydrothermal reaction, and the Ni3S4-MoS2 heterojunction material is obtained after a reactant is cooled, centrifugally washed and dried. The Ni3S4-MoS2 heterojunction material is used as the transduction layer of the all-solid-state sodium ion selective electrode, and the Ni3S4-MoS2 heterojunction material has excellent capacitance and hydrophobicity, so that the interface potential can be effectively stabilized, meanwhile, formation of a water layer on the surface of the electrode is inhibited, good potential response to sodium ions is realized, and the performance of the all-solid-state sodium ion selective electrode is improved. And excellent stability, reversibility and reproducibility are shown.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ion selective electrodes, and in particular to a Ni3S4-MoS2 heterojunction material and a preparation method and application thereof. Background Art

[0002] As a potentiometric electrochemical sensor, all-solid-state ion-selective electrodes are widely used in environmental monitoring and biomedicine due to their advantages such as fast response and high sensitivity. However, potential drift during long-term measurements and poor potential reproducibility of the electrode hinder its practical application. The solid contact layer in the all-solid-state ion-selective electrode is the transduction layer responsible for the mutual conversion of ion-electron signals. Its capacitance and hydrophobicity are key factors affecting the stability and performance of the electrode. Generally, all-solid-state ion-selective electrodes constructed based on large redox / double-layer capacitance and highly hydrophobic solid transduction layers have clear interface potentials, thereby exhibiting excellent electrochemical performance. Therefore, developing a new transduction layer with both excellent capacitance and hydrophobicity is a feasible strategy to ensure the potential stability and reproducibility of ion-selective electrodes.

[0003] As a transition metal sulfide, MoS2 is widely used in batteries, supercapacitors and other fields due to its unique layered structure and high theoretical capacity. However, its low conductivity and relatively few active sites limit its further application. Constructing metal sulfide-MoS2 heterojunctions through interface engineering can expose more active sites at the interface, thereby improving the catalytic performance of MoS2-based catalysts. Summary of the invention

[0004] The purpose of the present invention is to provide a Ni3S4-MoS2 heterojunction material, a preparation method and application thereof in an all-solid-state sodium ion selective electrode, so as to solve the problems of poor stability and poor reproducibility of the all-solid-state ion selective electrode in potential response.

[0005] The specific technical solutions of the present invention are as follows:

[0006] The preparation method of Ni3S4-MoS2 heterojunction material comprises the following steps:

[0007] S11, adding a molybdenum source, a nickel source and a sulfur source into water, and ultrasonically dispersing them to form a uniform mixed solution;

[0008] S12. The mixed solution is subjected to a hydrothermal reaction, and the reactants are cooled, centrifugally washed, and dried to obtain a Ni3S4-MoS2 heterojunction material.

[0009] In a further embodiment, the molybdenum source is at least one of sodium molybdate, potassium molybdate and ammonium molybdate;

[0010] The nickel source is at least one of nickel chloride, nickel nitrate and nickel acetate;

[0011] The sulfur source is at least one of thiourea and thioacetamide.

[0012] In a further embodiment, the molar ratio of the molybdenum source, the nickel source and the sulfur source is 2-4:1:10-15.

[0013] In a further embodiment, the temperature of the hydrothermal reaction is 180-220° C. and the time is 18-24 hours.

[0014] The second object of the present invention is to provide a Ni3S4-MoS2 heterojunction material prepared by the above preparation method.

[0015] The third invention object of the present invention is to provide an application of the above-mentioned Ni3S4-MoS2 heterojunction material, which is used as a transduction layer material in an all-solid-state sodium ion selective electrode.

[0016] In a further embodiment, the method for preparing the all-solid-state sodium ion selective electrode comprises the following steps:

[0017] S21, ultrasonically dispersing the Ni3S4-MoS2 heterojunction material in ethanol or deionized water to obtain a dispersion;

[0018] S22, dripping the dispersion onto the electrode surface and drying;

[0019] S23, drop-coating the sodium ion selective membrane solution on the top of the electrode treated in step S22, and drying, thereby obtaining an all-solid-state sodium ion selective electrode.

[0020] In a further embodiment, the electrode is a glassy carbon electrode or a screen-printed electrode;

[0021] In step S21, the concentration of the dispersion is 10 mg / mL.

[0022] Nickel-based sulfides are considered to be highly efficient electrocatalytic materials due to their excellent electrical conductivity. The introduction of transition metal Ni to construct heterojunction materials will redistribute the electrons of MoS2, thereby generating abundant active sites and improving electrical transfer efficiency and capacitance. At the same time, the introduction of Ni will also adjust the morphology of MoS2 to improve the hydrophobicity of the material. Therefore, the construction of Ni3S4-MoS2 heterojunction materials not only improves the capacitance of the material, but also adjusts the micromorphology of the material to improve the hydrophobicity. The sodium ion selective electrode constructed based on Ni3S4-MoS2 heterojunction material has excellent potential stability and reproducibility in potential response measurement.

[0023] Before coating the transfer layer material, the electrode in the all-solid-state sodium ion selective electrode needs to be pretreated. The pretreatment of the glassy carbon electrode is as follows: first, on a polishing cloth, the glassy carbon electrode is polished in 0.3μm and 0.05μm alumina dispersions, then ultrasonically cleaned in a solution of HNO3:H2O of 1:5, ethanol, and deionized water, and finally dried under an argon gas flow.

[0024] Preparation of sodium ion selective membrane solution: Sodium ion carrier X, sodium tetrakis[3,5-bis(trifluoromethyl)phenyl]borate (NaTFPB), dioctyl sebacate (DOS), and polyvinyl chloride (PVC) were dissolved in tetrahydrofuran (THF) and stirred at room temperature for three hours to obtain a transparent membrane mixed solution.

[0025] The present invention adopts a one-step hydrothermal method to prepare a Ni3S4-MoS2 heterojunction material. The construction of the heterojunction material not only increases the specific surface area of ​​the material, produces more abundant active sites, and improves the capacitance of the material, but also adjusts the morphology and structure of the material to increase the hydrophobicity of the material (capacitance: 208.3μF, contact angle: 115.6°).

[0026] The present invention uses Ni3S4-MoS2 heterojunction material as the transduction layer of the all-solid-state sodium ion selective electrode. Since Ni3S4-MoS2 heterojunction material has excellent capacitance and hydrophobicity, it can effectively stabilize the interface potential while inhibiting the formation of a water layer on the electrode surface, and exhibits good potential response, stability, reversibility and reproducibility to sodium ions. The Nernst slope is 57.95mV / dec, and the linear range is 10 -1 ~10 -5 M, detection limit: 10 -5.6 M, long-term stability: 11.34μV / h, relative standard deviation of the potential measurement of the same electrode: 2.14%, relative standard deviation of the potential measurement of different electrodes: 1.25%. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The scanning electron microscope and transmission electron microscope images of Ni3S4, MoS2 and Ni3S4-MoS2 prepared in Example 1 and Comparative Examples 1 and 2;

[0028] Figure 2 XRD and Raman spectra of Ni3S4, MoS2, and Ni3S4-MoS2;

[0029] Figure 3 BET and contact angle test diagrams of Ni3S4, MoS2, and Ni3S4-MoS2;

[0030] Figure 4Cyclic voltammetry curves and corresponding integral area diagrams of different loading concentrations of Ni3S4, MoS2, and Ni3S4-MoS2 materials;

[0031] Figure 5 For sodium ion selective electrode at 10 -1 -10 -9 Potential response diagram measured in 1M NaCl solution and the corresponding calibration curve;

[0032] Figure 6 Short-term and long-term stability measured for sodium ion selective electrodes;

[0033] Figure 7 For reproducibility measurement of sodium ion selective electrodes;

[0034] Figure 8 For reversibility, water layer and anti-interference tests of sodium ion selective electrodes. DETAILED DESCRIPTION

[0035] The present invention will be further explained below in conjunction with the embodiments and drawings, but the present invention is not limited thereto.

[0036] The reagents and materials used in the following examples are all commercially available products, and all reagents can be used directly without further purification.

[0037] Embodiment 1:

[0038] Dissolve 3.5mmol Na2MoO4·2H2O, 1mmol NiCl2·6H2O, and 15mmol CH4N2S in 30mL deionized water and disperse by ultrasonic to form a uniform mixed solution;

[0039] The mixed solution was transferred to a 50 mL polytetrafluoroethylene-lined stainless steel autoclave and heated at 180°C for 24 h for a hydrothermal reaction; the reactants were cooled, washed three times by centrifugation with water and ethanol respectively, and then vacuum dried at 60°C to obtain a Ni3S4-MoS2 heterojunction material.

[0040] Embodiment 2:

[0041] Dissolve 4 mmol of ammonium molybdate, 1 mmol of nickel acetate, and 10 mmol of thioacetamide in 30 mL of deionized water, and disperse by ultrasonication to form a uniform mixed solution;

[0042] The mixed solution was transferred to a 50 mL polytetrafluoroethylene-lined stainless steel autoclave and heated at 220 °C for 18 h for hydrothermal reaction. The reactants were cooled, and the precipitates were washed three times by centrifugation with water and ethanol, respectively. Finally, the precipitates were collected and dried in vacuum at 60 °C to obtain Ni3S4-MoS2 materials.

[0043] Embodiment 3:

[0044] The preparation process of the all-solid-state sodium ion selective electrode is as follows:

[0045] Preparation of transduction layer material: 2mmol K2MoO4, 1mmol Ni(NO3)2·6H2O, and 12mmol CH4N2S were dissolved in 30mL deionized water and dispersed by ultrasonic to form a uniform mixture. The mixture was transferred to a 50mL polytetrafluoroethylene-lined stainless steel autoclave and heated at 200℃ for 20h for hydrothermal reaction. After cooling, the precipitate was washed three times by centrifugation with water and ethanol respectively, and finally the precipitate was collected and vacuum dried at 60℃ to obtain Ni3S4-MoS2 material.

[0046] Preparation of sodium ion selective membrane solution: 1 wt% sodium ion carrier X, 0.6 wt% sodium tetrakis[3,5-bis(trifluoromethyl)phenyl]borate, 65.4 wt% dioctyl sebacate and 33 wt% polyvinyl chloride (250 mg in total) were dissolved in 2.5 mL tetrahydrofuran and stirred at room temperature in a fume hood to a transparent solution.

[0047] Pretreatment of glassy carbon electrode: First, on a polishing cloth, polish the glassy carbon electrode in 0.3μm and 0.05μm alumina dispersions, then ultrasonically clean it in a solution of HNO3:H2O with a ratio of 1:5, ethanol, and deionized water, and finally dry it under an argon gas flow for use.

[0048] Construction of all-solid-state sodium ion selective electrode:

[0049] ① Preparation of GC / Ni3S4-MoS2: Weigh the Ni3S4-MoS2 material prepared in Example 1 and disperse it in 1 mL of deionized water. Ultrasonic disperse it evenly to prepare Ni3S4-MoS2 dispersions of different concentrations (8 concentrations: 6, 8, 10, 12, 14, 16, 18, 20 mg / mL). Use a pipette to take 5 μL of each of the above 8 concentrations of dispersion, and then add them dropwise to the pretreated glassy carbon electrode surface, and dry at room temperature to obtain GC / Ni3S4-MoS2.

[0050] ②GC / Ni3S4-MoS2 / Na + - Preparation of ISE: Use a pipette to take 10 μL each time, and apply 100 μL of sodium ion selective membrane solution on the top of the GC / Ni3S4-MoS2 electrode in batches, and then place it in a fume hood at room temperature to dry for 12 hours to obtain an all-solid-state sodium ion selective electrode.

[0051] Comparative Example 1:

[0052] 3.5mmol Na2MoO4·2H2O and 15mmol CH4N2S were dissolved in 30mL deionized water and ultrasonically dispersed to form a uniform mixed solution;

[0053] The mixed solution was transferred to a 50 mL polytetrafluoroethylene-lined stainless steel autoclave and heated at 180 °C for 24 h for a hydrothermal reaction; the reactants were cooled, washed three times by centrifugation with water and ethanol respectively, and then vacuum dried at 60 °C to obtain MoS2 material.

[0054] Comparative Example 2:

[0055] 1.5 mmol NiCl2·6H2O and 10 mmol CH4N2O (urea) were dissolved in 30 mL deionized water and dispersed by ultrasonic to form a uniform solution.

[0056] The mixture was transferred into a 50 mL polytetrafluoroethylene-lined stainless steel autoclave and heated at 130 °C for 2 h for a hydrothermal reaction; the reactants were cooled, washed three times with water and ethanol by centrifugation, respectively, and then dried in vacuo at 60 °C to obtain a Ni(OH)2 precursor.

[0057] The Ni(OH)2 precursor and 15mmol Na2S·9H2O were dissolved in 30mL deionized water, transferred to a 50mL polytetrafluoroethylene-lined stainless steel autoclave, reacted at 90°C for 9h, and the obtained precipitate was washed three times by centrifugation with water and ethanol respectively. Finally, the precipitate was collected and vacuum dried at 60°C for 12h to obtain Ni3S4 material.

[0058] Comparative Example 3:

[0059] Using the MoS2 material and Ni3S4 material prepared in Comparative Examples 1 and 2, GC / Ni3S4 and GC / MoS2, GC / Ni3S4 / Na3S4 were prepared according to the steps in Example 3. + -ISE and GC / MoS2 / Na + -ISE.

[0060] Test Example 1:

[0061] The materials prepared in the above-mentioned Example 1 and Comparative Examples 1-2 were subjected to relevant performance tests, and the test methods were as follows:

[0062] Scanning electron microscopy (SEM, Sirion200, FEI) and high-resolution transmission electron microscopy (HRTEM, JEM-2010, JEOL) were used to characterize the morphology of the materials.

[0063] Use PANalytical X-ray diffractometer to characterize the crystal form and structural characteristics of the material;

[0064] Raman spectra of the materials were collected using a Raman spectrometer (LabRAM HR800);

[0065] The specific surface area of ​​the materials was determined by the Brunauer-Emmett-Teller (BET) N2 adsorption-desorption method using an automatic specific surface area measurement device (Tristar II 3020M, Micromeritics, USA);

[0066] The contact angle of the material was measured using a high temperature contact angle meter (DSAHT17C);

[0067] All electrochemical tests were measured using an electrochemical workstation (CHI760E, Shanghai Chenhua).

[0068] The specific test objects and test results are as follows:

[0069] The Ni3S4-MoS2, MoS2, and Ni3S4 materials prepared in Example 1 and Comparative Examples 1 and 2 were subjected to scanning electron microscopy, transmission electron microscopy, X-ray diffraction, Raman spectroscopy, BET specific surface area, and contact angle tests, and the results are shown in Figure 1-3 .

[0070] Figure 1 Ac are scanning electron microscope images, where a is the scanning electron microscope image of the Ni3S4 material prepared in Comparative Example 2, b is the scanning electron microscope image of the MoS2 material prepared in Comparative Example 1, and c is the scanning electron microscope image of the Ni3S4-MoS2 heterojunction material prepared in Example 1.

[0071] Figure 1 In the figure, d and f are transmission electron microscope images, wherein d is the transmission electron microscope image of the Ni3S4 material prepared in comparative example 2, e is the transmission electron microscope image of the MoS2 material prepared in comparative example 1, and f is the transmission electron microscope image of the Ni3S4-MoS2 heterojunction material prepared in example 1.

[0072] Depend on Figure 1 The scanning electron microscope image shows that Ni3S4-MoS2 is a hierarchical nanosphere composed of nanosheets. Figure 1 In parts b and c, it can be found that due to the introduction of Ni3S4, the nanosheets of Ni3S4-MoS2 are larger than those of MoS2.

[0073] Transmission electron microscopy images provide further microstructure of the Ni3S4-MoS2 heterojunction material. Figure 1In the df, the lattice spacing of 0.16 nm in Ni3S4-MoS2 corresponds to the (440) crystal plane of Ni3S4, and the lattice spacing of 0.27 nm corresponds to the (100) crystal plane of MoS2, indicating that the product prepared in Example 1 is composed of Ni3S4 and MoS2. At the same time, the (100) crystal plane of MoS2 and the (440) crystal plane of Ni3S4 constitute an important heterogeneous interface in the composite material, proving that the Ni3S4-MoS2 heterojunction material was successfully prepared.

[0074] Figure 2 Figure a is the XRD spectrum of Ni3S4-MoS2, MoS2, and Ni3S4 materials. It can be seen from the figure that Ni3S4-MoS2 has the characteristic peaks of both MoS2 and Ni3S4, among which the characteristic peaks of 14.3°, 32.8°, and 58.7° correspond to the (002), (100), and (110) crystal planes of MoS2 phase (XRD spectrum standard card JCPDS#37-1492), respectively; the peaks of 26.6°, 31.3°, 38.1°, 49.9°, and 54.6° correspond to the (220), (311), (400), (511), and (440) crystal planes of Ni3S4 phase (XRD spectrum standard card JCPDS#47-1739), respectively.

[0075] Figure 2 Figure b is the Raman spectrum of the material. The vibration modes of Ni3S4 and MoS2 exist simultaneously in the Ni3S4-MoS2 heterojunction material, further indicating that the Ni3S4-MoS2 heterojunction material was successfully prepared.

[0076] Figure 3 In the above equation, ac is Ni3S 4、 From the BET specific surface area test diagram of MoS2 and Ni3S4-MoS2, it can be seen that Ni3S 4、 MoS2、Ni3S4-MoS 24 The surface areas are 3.6, 6.5 and 39.2 m 2 / g, indicating that the construction of Ni3S4-MoS2 heterojunction increases the surface area of ​​the sample.

[0077] Figure 3 Where d is Ni3S 4、 From the contact angle tests of MoS2 and Ni3S4-MoS2, it can be seen that the introduction of Ni3S4 in Ni3S4-MoS2 also increases the hydrophobicity of the material, and its contact angle reaches 115.6°.

[0078] Test Example 2:

[0079] A glassy carbon electrode was used as the working electrode, a platinum wire electrode was used as the counter electrode, and Ag / AgCl (3 mol / L KCl) was used as the reference electrode to form a three-electrode system. Using a CHI760E electrochemical workstation (Shanghai Chenhua Instrument Co., Ltd., China), GC / Ni3S4 (such as Figure 4 As shown in ab), GC / MoS2 (as shown in Figure 4 cd) and GC / Ni3S4-MoS2 in Example 3 (as shown in Figure 4 Cyclic voltammetry (CV) tests were performed on the samples (shown in Figure ef).

[0080] from Figure 4 It can be seen that GC / Ni3S4-MoS2 has the largest current area, indicating that it has the largest capacitance, indicating that the construction of its heterojunction exposes more active sites, improving the electrical transfer efficiency and capacitance. At the same time, the CV curves under different dispersion concentrations show that when the concentrations of Ni3S4, MoS2, and Ni3S4-MoS2 are 12, 14, and 10 mg / mL, respectively, the current area reaches the maximum, so the above concentrations are selected as the optimal concentrations of the subsequent (Test Example 3) all-solid-state sodium ion selective electrode transduction layer.

[0081] Test Example 3:

[0082] The electrode GC / Ni3S4-MoS2 / Na2O3 was constructed with the optimal concentration of the transfer layer in Experiment 2. + -ISE、GC / Ni3S4 / Na + -ISE and GC / MoS2 / Na + -ISE, a series of electrochemical tests were performed. Before the potential response measurement, the electrode was first -3 MNaCl solution for one day, and then -9 M NaCl solution for two days; for the other tests, the electrodes were activated at 10 -3 Activate in M ​​NaCl solution overnight. The details are as follows:

[0083] Open circuit potential test:

[0084] Using the open circuit potential, the Na + Perform dynamic potential measurements, such as Figure 5 As shown in the figure, the measured potential response diagram and the corresponding calibration curve are shown. + -ISE (eg Figure 5 (a, d), GC / MoS2 / Na + -ISE (eg Figure 5 b, e) and GC / Ni3S4-MoS2 / Na+ -ISE (eg Figure 5 (c, f) for Na + The Nernst slopes of the detection were 56.48, 55.23, and 57.95 mV / dec, and the detection limits were 10 -4.9 , 10 -4.6 , 10 -5.6 M, Na that achieves a near-Nernstian response + Low level detection.

[0085] Short-term and long-term stability:

[0086] The short-term stability of the electrode was evaluated by chronopotentiometry. Figure 6 As shown in a, GC / Ni3S4 / Na + -ISE、GC / MoS2 / Na + -ISE and GC / Ni3S4-MoS2 / Na + The short-term potential drift values ​​of -ISE were 20.2, 6.9, and 4.8 μV / s, respectively. The long-term stability was evaluated by measuring the long-term open circuit potential of the electrode in 0.1 M NaCl solution. The results are shown in Figure 6 Medium b, GC / Ni3S4 / Na + -ISE、GC / MoS2 / Na + -ISE and GC / Ni3S4-MoS2 / Na + -ISE short-term potential drift values ​​are 30.2, 23.4, and 11.3 μV / h, respectively. + -ISE has the best short-term and long-term stability, which is attributed to the higher capacitance and hydrophobicity of the Ni3S4-MoS2 heterojunction.

[0087] Reproducibility test:

[0088] By measuring a GC / Ni3S4-MoS2 / Na + -ISE electrode at 10 -1 -10 -4 Ten potential responses in M ​​NaCl solution (such as Figure 7 ) and the potential responses of ten different electrodes (as shown in Figure 7 The standard deviations of the Nernst slopes were 2.14% and 1.25%, respectively, indicating that the GC / Ni3S4-MoS2 / Na + -ISE electrodes have good reproducibility.

[0089] Reversibility, water layer and anti-interference tests:

[0090] GC / Ni3S4-MoS2 / Na + -ISE electrodes are immersed in succession for 10 -1 , 10 -2 , 10 -3 The electrode potential was measured in M ​​NaCl solution to evaluate the reversibility of the electrode. Figure 8 As shown in a, when GC / Ni3S4-MoS2 / Na + When the -ISE electrode was alternately measured in different solutions, the potential response was stable and there was no obvious potential fluctuation, indicating that the electrode had excellent reversibility.

[0091] GC / Ni3S4-MoS2 / Na + -ISE electrodes are immersed in 10 -1 M NaCl solution and 10 -1 M KCl solution to perform water layer tests, such as Figure 8 As shown in b, GC / Ni3S4-MoS2 / Na + The -ISE electrode did not have obvious potential drift during the water layer test, indicating that there was no water layer between Ni3S4-MoS2 and the ion selective membrane, which was attributed to the high hydrophobicity of the Ni3S4-MoS2 heterojunction.

[0092] In addition, the electrode also has excellent resistance to light, N2, O2, CO2 interference performance such as Figure 8 As shown in c.

[0093] The above description of the embodiments is to facilitate the understanding and application of the present invention by those skilled in the art. It is obvious that those familiar with the art can easily make various modifications to the implementation cases and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the implementation cases here, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A method for preparing a Ni3S4-MoS2 heterojunction material, characterized in that: The following steps are involved: S11, adding a molybdenum source, a nickel source and a sulfur source into water, and ultrasonically dispersing them to form a uniform mixed solution; S12. The mixed solution is subjected to a hydrothermal reaction, and the reactants are cooled, centrifugally washed, and dried to obtain a Ni3S4-MoS2 heterojunction material.

2. The preparation method according to claim 1, characterized in that: The molybdenum source is at least one of sodium molybdate, potassium molybdate and ammonium molybdate; The nickel source is at least one of nickel chloride, nickel nitrate and nickel acetate; The sulfur source is at least one of thiourea and thioacetamide.

3. The preparation method according to claim 1, characterized in that: The molar ratio of the molybdenum source, the nickel source and the sulfur source is 2-4:1:10-15.

4. The preparation method according to claim 1, characterized in that: The temperature of the hydrothermal reaction is 180-220° C. and the time is 18-24 hours.

5. The Ni3S4-MoS2 heterojunction material obtained by the preparation method according to any one of claims 1 to 4.

6. The use of the Ni3S4-MoS2 heterojunction material as claimed in claim 5, characterized in that: It is used as a transduction layer material in all-solid-state sodium ion selective electrodes.

7. The use according to claim 6, characterized in that: The preparation method of the all-solid-state sodium ion selective electrode comprises the following steps: S21, ultrasonically dispersing the Ni3S4-MoS2 heterojunction material in ethanol or deionized water to obtain a dispersion; S22, dripping the dispersion onto the electrode surface and drying; S23, drop-coating the sodium ion selective membrane solution on the top of the electrode treated in step S22, and drying, thereby obtaining an all-solid-state sodium ion selective electrode.

8. The use according to claim 7, characterized in that: The electrode is a glassy carbon electrode or a screen-printed electrode; In step S21, the concentration of the dispersion is 10 mg / mL.

Citation Information

Cited By

  • Se-doped CuCo2S4 composite material, all-solid-state sodium ion selective electrode and preparation method and application of all-solid-state sodium ion selective electrode

    CN122301137A