Slow-release composite sulfur autotrophic denitrification filler as well as preparation method and application thereof

Through the sustained-release composite sulfur autotrophic denitrification filler, the use of sulfur powder, ferrous sulfide and other components, combined with composite calcium carbonate and bentonite, the problems of poor nitrogen removal effect and serious filler loss in wastewater treatment are solved, and the problem of Efficient nitrate nitrogen removal and stable pH value reduce wastewater treatment costs.

CN119038745AActive Publication Date: 2024-11-29HUNAN CHENGTONG TIANYUE ENV PROTECTION TECH CO LTD

Patent Information

Application Number
CN202411348394.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-11-29
Estimated Expiration
2044-09-26

AI Technical Summary

Technical Problem

Municipal sewage plants need a large number of carbon sources to achieve denitrification during the biological denitrification process, resulting in high operating costs, and the existing sulfur autotrophic denitrification fillers have poor denitrification effects, severe filler loss, and insufficient system pH buffering effect.

Method used

Use sustained-release composite sulfur autotrophic denitrification fillers, including sulfur powder, ferrous sulfide, compound calcium carbonate, sodium bentonite, corn starch and adhesives, and are prepared through granulation process to treat wastewater and improve nitrogen removal effect and pH Value stability.

Benefits of technology

An efficient nitrate nitrogen removal rate (more than 96%) is achieved, which reduces filler loss and operating costs, keeps the effluent pH value tending to be neutral, has high filler strength, and reduces the need for additional carbon source injection and pH adjustment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention belongs to the technical field of sewage treatment, and particularly relates to slow-release type composite sulfur autotrophic denitrification filler, a preparation method and application thereof.The slow-release type composite sulfur autotrophic denitrification filler is prepared from, by weight, 4-6 parts of sulfur powder, 1-3 parts of ferrous sulfide, 1-3 parts of pH buffering agent, 0.5-1.5 parts of bentonite, 0.5-1.5 parts of starch and 0.5-1.5 parts of adhesive. The filler loss and the cost are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sewage treatment, and in particular relates to a slow-release composite sulfur autotrophic denitrification filler, a preparation method and an application thereof. Background Art

[0002] As environmental protection policies become increasingly stringent, it is imperative to improve the municipal sewage pollutant discharge standards, and the demand for deep denitrification of tailwater is also growing. In order to achieve the best denitrification effect in the heterotrophic denitrification process of biological denitrification, a large amount of carbon source needs to be consumed. However, the secondary effluent of general municipal sewage treatment plants has less carbon source for denitrification, and a large amount of carbon source needs to be added to meet the reaction conditions, which will lead to excessively high operating costs of sewage treatment plants. This requires the use of sulfur autotrophic denitrification process to treat total nitrogen, but the common sulfur autotrophic denitrification fillers on the market have problems such as poor denitrification effect, serious filler loss, poor system pH buffering effect, and high cost.

[0003] Patent application publication number CN115028261A discloses a sulfur autotrophic denitrification filler and a preparation method thereof. The sulfur autotrophic denitrification filler comprises the following components in parts by weight: 50 to 100 parts of sulfur powder, 1 to 10 parts of an alkaline reducing agent, 10 to 40 parts of a pH buffer, 10 to 50 parts of kaolin and 10 to 20 parts of a binder; wherein the alkaline reducing agent is a sulfite or a bisulfite. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a slow-release composite sulfur autotrophic denitrification filler, a preparation method and an application thereof, so as to improve the denitrification effect, make the pH value of the effluent more neutral, reduce the loss of the filler and reduce the cost.

[0005] The embodiment of the present invention provides a slow-release composite sulfur autotrophic denitrification filler, comprising the following components in parts by weight: 4-6 parts of sulfur powder, 1-3 parts of ferrous sulfide, 1-3 parts of pH buffer, 0.5-1.5 parts of bentonite, 0.5-1.5 parts of starch, and 0.5-1.5 parts of adhesive.

[0006] Preferably, the composition comprises the following components in parts by weight: 4 parts of sulfur powder, 1 part of ferrous sulfide, 2 parts of pH buffer, 1 part of bentonite, 1 part of starch and 1 part of adhesive.

[0007] Preferably, the particle size of the sulfur powder is 150-200 mesh.

[0008] Preferably, the pH buffer is a composite calcium carbonate, which includes the following weight percentage components: 45-55% light calcium carbonate, 35-45% nano calcium carbonate, and 5-15% sodium chlorate (preferably 50% light calcium carbonate, 40% nano calcium carbonate, and 10% sodium chlorate). Composite calcium carbonate can effectively solve the problem of a significant decrease in system pH during sulfur autotrophic denitrification.

[0009] Preferably, the bentonite is one or more of sodium-based bentonite, calcium-based bentonite, and magnesium-based bentonite. Bentonite can regulate the pH of the system during sulfur autotrophic denitrification and improve the strength of the filler. Preferably, the starch is corn starch.

[0010] Preferably, the adhesive is one or more of styrene and butyl acrylate.

[0011] Preferably, the particle size of the slow-release composite sulfur autotrophic denitrification filler is 8-10 mm, and the bulk density is 1.13-1.28 g / cm 3 .

[0012] The embodiment of the present invention provides a method for preparing the slow-release composite sulfur autotrophic denitrification filler. Sulfur powder, ferrous sulfide, pH buffer, bentonite and starch are mixed and granulated. An adhesive is sprayed during the granulation process. After the granulation is completed, the mixture is dried, cooled and sieved to obtain the slow-release composite sulfur autotrophic denitrification filler.

[0013] The specific preparation method is as follows: sulfur powder, ferrous sulfide, pH buffer, bentonite and starch are screened, the screened raw materials are mixed in a stirrer according to a proportion, the mixing time is 20 minutes, the mixed raw materials are slowly added to a disc granulator, the adhesive and water are mixed in a volume ratio of 1:2-4, and the mixed raw materials are evenly sprayed into the disc granulator, and the adhesive diluent is sprayed while feeding to perform granulation. After the granulation is completed, the spraying of the adhesive diluent is stopped, and the filler continues to roll in the disc granulator for 5-10 minutes. After the rolling is completed, it is heated and dried at a temperature of 70-95°C. After the drying is completed, it is cooled and screened to obtain the slow-release composite sulfur autotrophic denitrification filler.

[0014] The embodiment of the present invention provides an application of the slow-release composite sulfur autotrophic denitrification filler, and the slow-release composite sulfur autotrophic denitrification filler is used for treating sewage.

[0015] The beneficial effect of the present invention is that the present invention uses composite calcium carbonate as a buffer, which can effectively solve the problem of a significant decrease in the system pH during the sulfur autotrophic denitrification process. The present invention uses one or more of sodium-based bentonite, calcium-based bentonite, and magnesium-based bentonite, which can regulate the system pH during the sulfur autotrophic denitrification process and improve the filler strength. In the present invention, the adhesive and water are mixed in a volume ratio of 1:2 to 4, so that the spraying device of the disc granulator is not easy to be blocked, and at the same time, it is beneficial to higher filler strength and better sustained release effect. The present invention uses a disc granulator for granulation, and no toxic and harmful gases are generated during the granulation process. The operation is convenient, the molding is easy, and the production cost is low.

[0016] The sulfur autotrophic denitrification filler prepared by the present invention is a slow-release denitrification filler, which uses the sulfur in the filler as an electron donor to reduce the nitrate nitrogen in the water body to N 2 , thus achieving the purpose of purifying water quality. The filler has high nitrate nitrogen removal efficiency, with a removal rate of more than 96%, good slow-release effect, no need to add additional carbon source, no need to adjust the system pH, high filler strength, low replenishment frequency, greatly saving sewage treatment costs.

[0017] The present invention selects ferrous sulfide as a reducing agent, composite calcium carbonate as a pH buffer, and also includes corn starch and styrene, which significantly improves the removal rate of nitrate nitrogen and keeps the pH value of the effluent more neutral, and the strength of the filler is higher, so that the loss of the filler is less. DETAILED DESCRIPTION

[0018] The present invention is specifically described below according to specific embodiments: The present invention provides a deep denitrification filler and a preparation method thereof to solve the problems of poor denitrification effect, serious filler loss, poor system pH buffering effect, and high cost. The technical scheme in the embodiment of the present invention is clearly and completely described below. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0019] Example 1 A method for preparing a slow-release composite sulfur autotrophic denitrification filler comprises the following steps: Firstly, sulfur powder, ferrous sulfide, composite calcium carbonate (including the following weight percentage components, light calcium carbonate 50%, nano calcium carbonate 40%, sodium chlorate 10%), sodium bentonite powder and corn starch with a particle size of 200 mesh are sieved and filtered, and the filtered raw materials are mixed in a blender at a mass ratio of 4:1:2:1:1 for 20 minutes. The mixed raw materials are slowly added into a disc granulator, and styrene (the weight ratio of styrene to corn starch is 1:1) and water are mixed at a volume ratio of 1:4. After mixing, they are evenly sprayed into the disc granulator, and the adhesive diluent is sprayed while feeding to perform granulation. After the granulation is completed, the spraying of the adhesive diluent is stopped, and the filler continues to roll in the disc granulator for 10 minutes. After the rolling is completed, it is heated and dried at 75°C. After the drying is completed, it is cooled and screened to obtain the final product.

[0020] Example 2 A method for preparing a slow-release composite sulfur autotrophic denitrification filler comprises the following steps: Firstly, sulfur powder, ferrous sulfide, composite calcium carbonate (including the following weight percentage components, light calcium carbonate 50%, nano calcium carbonate 40%, sodium chlorate 10%), calcium-based bentonite powder and corn starch with a particle size of 200 mesh are sieved and filtered, and the filtered raw materials are mixed in a blender according to a mass ratio of 5:3:1:1.5:0.5 for 30 minutes. The mixed raw materials are slowly added into a disc granulator, and butyl acrylate (the weight ratio of butyl acrylate and corn starch is 1:1) and water are mixed in a volume ratio of 1:4. After mixing, they are evenly sprayed into the disc granulator, and the adhesive diluent is sprayed while feeding to granulate. After the granulation is completed, the spraying of the adhesive diluent is stopped, and the filler continues to roll in the disc granulator for 10 minutes. After the rolling is completed, it is heated and dried at 90°C. After the drying is completed, it is cooled and sieved to obtain the final product.

[0021] Comparative Example 1 Compared with Example 1, the difference is that ferrous sulfide is replaced by sodium sulfite, and the rest is the same as Example 1.

[0022] Comparative Example 2 Compared with Example 1, the difference is that the composite calcium carbonate is replaced by sodium carbonate, and the rest is the same as Example 1.

[0023] Comparative Example 3 Compared with Example 1, the difference is that corn starch is replaced by kaolin, and the rest is the same as Example 1.

[0024] Comparative Example 4 Compared with Example 1, the difference is that styrene is replaced by carboxymethyl cellulose, and the rest is the same as Example 1.

[0025] Example 3 1 kg of each of the slow-release composite sulfur autotrophic denitrification fillers prepared in Examples 1-2 and Comparative Examples 1-4 were used for a sulfur autotrophic denitrification comparative experiment to compare and analyze the denitrification effect, pH buffering effect, and filler strength change.

[0026] Experimental content: The experimental water sample is the effluent from the secondary sedimentation tank of the municipal sewage treatment plant, with a nitrate nitrogen concentration of 10~15 mg / L and a pH of 6.85~7.0.

[0027] 1 kg of the slow-release composite sulfur autotrophic denitrification filler prepared in each embodiment was placed in a denitrification column as an experimental group, and 1 kg of the slow-release composite sulfur autotrophic denitrification filler in each comparative example was placed in a denitrification column as a control group. 20 mL of aeration tank activated sludge was added to each denitrification column, and then the sewage from the secondary sedimentation tank was introduced for circulating biofilm cultivation. The water temperature was controlled to be 25°C. After three days, a continuous inlet and outlet water experiment was started, and the HRT was 0.5 h. After completing three days of biofilm cultivation, the nitrate nitrogen concentration was detected daily. The results of the continuous inlet and outlet water experiment are shown in Tables 1-3.

[0028] Table 1 Nitrate nitrogen removal

[0029] Table 2 Changes in pH of inlet and outlet water

[0030] Table 3 Changes in packing cylinder pressure strength

[0031] The experimental results show that the average removal rates of nitrate nitrogen in Examples 1 and 2 are 96% and 97%, respectively, while in the control group, the average removal rates of nitrate nitrogen in Comparative Examples 1-4 are 67%, 77%, 72% and 81%, respectively.

[0032] The average nitrate nitrogen removal rate is calculated as the average value of the nitrate nitrogen removal rates from the 1st to the 5th day. The nitrate nitrogen removal rate is calculated as the removed nitrate nitrogen / the influent nitrate nitrogen on that day. For example, the nitrate nitrogen removal rate on the first day is (13.4-0.6) / 13.4*100%=96%.

[0033] The pH of the effluent from the experimental group was stable at around 6.8, while the pH of the effluent from the control group fluctuated greatly, with the average pH of the effluent from comparative examples 1-4 being between 6.1 and 6.7.

[0034] After the experiment, the two fillers were tested for strength. Five fillers were randomly selected for strength testing in each group of experiments, and the test results were calculated as average values. The test results showed that the average cylinder pressure strengths of Example 1 and Example 2 were 6.97 MPa, respectively. In the control group, the average cylinder pressure strengths of Comparative Examples 1-4 were 6.97 MPa, 6.87 MPa, 6.66 MPa, 5.49 MPa, and 4.51 MPa, respectively. It can be seen that the prepared slow-release composite sulfur autotrophic denitrification filler has a significantly better denitrification effect, pH buffering capacity, and filler strength than the comparative sulfur autotrophic denitrification filler.

[0035] A person skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of protection of the present application is limited to these examples. In line with the concept of the present application, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of different aspects of one or more embodiments of the present application as described above, which are not provided in detail for the sake of simplicity.

[0036] One or more embodiments of the present application are intended to cover all such substitutions, modifications and variations that fall within the broad scope of the present application. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of one or more embodiments of the present application should be included in the protection scope of the present application.

Claims

1. A slow-release composite sulfur autotrophic denitrification filler, characterized in that it includes The components are as follows in parts by weight: 4-6 parts of sulfur powder, 1-3 parts of ferrous sulfide, 1-3 parts of pH buffer, 0.5-1.5 parts of bentonite, 0.5-1.5 parts of starch, and 0.5-1.5 parts of adhesive.

2. The slow-release composite sulfur autotrophic denitrification filler according to claim 1, characterized in that it comprises The components are as follows in parts by weight: 4 parts of sulfur powder, 1 part of ferrous sulfide, 2 parts of pH buffer, 1 part of bentonite, 1 part of starch, and 1 part of adhesive.

3. The slow-release composite sulfur autotrophic denitrification filler according to claim 1 or 2, characterized in that: The particle size of the sulfur powder is 150-200 meshes.

4. The slow-release composite sulfur autotrophic denitrification filler according to claim 1 or 2, characterized in that: The pH buffer is composite calcium carbonate, which includes the following components in percentage by weight: 45-55% light calcium carbonate, 35-45% nano calcium carbonate, and 5-15% sodium chlorate.

5. The slow-release composite sulfur autotrophic denitrification filler according to claim 1 or 2, characterized in that: The bentonite is one or more of sodium-based bentonite, calcium-based bentonite and magnesium-based bentonite.

6. The slow-release composite sulfur autotrophic denitrification filler according to claim 1 or 2, characterized in that: The starch is corn starch.

7. The slow-release composite sulfur autotrophic denitrification filler according to claim 1 or 2, characterized in that: The adhesive is one or more of styrene and butyl acrylate.

8. The slow-release composite sulfur autotrophic denitrification filler according to claim 1 or 2, characterized in that: The particle size of the slow-release composite sulfur autotrophic denitrification filler is 8-10 mm, and the bulk density is 1.13-1.28 g / cm 3 .

9. A method for preparing a slow-release composite sulfur autotrophic denitrification filler as claimed in any one of claims 1 to 8, characterized in that: Sulfur powder, ferrous sulfide, pH buffer, bentonite and starch are mixed and granulated, and an adhesive is sprayed during the granulation process. After the granulation is completed, the mixture is dried, cooled and sieved to obtain a slow-release composite sulfur autotrophic denitrification filler.

10. An application of the slow-release composite sulfur autotrophic denitrification filler according to any one of claims 1 to 8, characterized in that: The slow-release composite sulfur autotrophic denitrification filler is used for treating sewage.

Citation Information

Patent Citations

  • Sulfur autotrophic filler as well as preparation method and application thereof

    CN116143281A

  • Solid-phase slow-release sulfur filler based on sulfur autotrophic nitrogen removal as well as preparation method and application of solid-phase slow-release sulfur filler

    CN116605986A

  • MXene enhanced ferrous sulfide autotrophic denitrification composite filler as well as preparation method and application thereof

    CN117602735A

  • Sulfur autotrophic denitrification filler and preparation method thereof

    CN118359322A

  • Biological carrier material with sulfur autotrophic denitrification function as well as preparation method and application of biological carrier material

    CN118598360A

Cited By

  • Autotrophic denitrification filler for denitrification and preparation method thereof

    CN119524790A