Carbon-nitrogen co-doped NiO electrochromic film, intelligent window and preparation method of carbon-nitrogen co-doped NiO electrochromic film

By using a carbon-nitrogen co-doped NiO electrochromic thin film preparation method, the problems of complex preparation process and high cost of nickel oxide electrochromic materials have been solved, achieving efficient and environmentally friendly electrochromic performance and stability, which is suitable for applications such as building energy-saving windows.

CN119038887AActive Publication Date: 2024-11-29SHANGHAI UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411143467.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-29
Estimated Expiration
2044-08-20

AI Technical Summary

Technical Problem

Existing nickel oxide electrochromic materials have complex preparation processes, high costs, and poor film uniformity, making it difficult to meet the requirements for large-scale applications.

Method used

A method for preparing carbon-nitrogen co-doped NiO electrochromic thin films was adopted. Ethanolamine was added to a nickel salt solution as a chelating agent and modifier. The film was then sprayed onto the substrate surface and subjected to heat treatment to form a uniform carbon-nitrogen co-doped NiO thin film. The film was then assembled with conductive glass to form a smart window.

Benefits of technology

It improves the conductivity and electrochromic properties of NiO films, enhances cycle stability, reduces production costs, and is suitable for large-scale production and application. Furthermore, the use of environmentally friendly solvents reduces harmful gas emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038887A_ABST
    Figure CN119038887A_ABST
Patent Text Reader

Abstract

The invention discloses a carbon and nitrogen co-doped NiO electrochromic film, an intelligent window and a preparation method of the carbon and nitrogen co-doped NiO electrochromic film, and belongs to the technical field of electrochromic intelligent devices.The preparation method comprises the steps that nickel salt is dissolved in absolute ethyl alcohol, ethanolamine is added, stirring is performed to form a nickel salt solution, the nickel salt solution is sprayed to the surface of a base body, the carbon and nitrogen co-doped NiO electrochromic film is obtained through curing, and the carbon and nitrogen co-doped NiO electrochromic film is obtained. The carbon and nitrogen co-doped NiO can improve the conductivity of the material, so that the NiO film has higher coloring efficiency, higher response speed and good light adjusting performance. Meanwhile, the amorphous crystal structure can avoid structural collapse caused by volume expansion, so that the cycling stability is improved, and the material is suitable for the fields of building energy-saving windows and the like and has wide market prospects and application potential.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of electrochromic smart devices, and in particular relates to a carbon-nitrogen co-doped NiO electrochromic film and a smart window and a preparation method thereof. Background Art

[0002] Electrochromic technology has received extensive attention in the field of building energy conservation in recent years. Due to its large spectral modulation amplitude, high coloring efficiency, fast response speed, and ability to be actively or at any time regulated, it is widely considered to be the best solution for the preparation of smart energy-saving windows.

[0003] Nickel oxide (NiO) is a commonly used electrochromic positive electrode material. When a forward voltage is applied, the film changes from transparent to brown; when a reverse voltage is applied, the film returns to a transparent state. NiO crystals have a cubic structure similar to that of NaCl, and the lattice is tightly arranged, which is not conducive to the insertion and removal of electrolyte ions. Therefore, its electrochromic cycle stability is poor. Researchers have adopted a series of strategies to improve its various performance indicators, including element doping, conductive material coating, micromorphology regulation, electrolyte ion selection, porous / mesoporous / amorphous structure design, and synthesis of quantum dots. For example, the literature (Materials Chemistry and Physics 306 (2023) 128079) discloses a Sn-doped amorphous NiO. Due to Sn 4+ Replaced part of Ni 2+ , Ni vacancies increase, and part of Ni 2+ Easier to convert to Ni 3+ , effectively accelerating the electron transfer rate, while the cycle life is increased to 30,000 times. The preparation of high-quality electrochromic films requires providing a good diffusion channel for electron ions, and the pores between particles can effectively accommodate volume expansion. However, most nickel oxide electrochromic materials currently cannot meet this requirement. At the same time, the preparation of thin films generally adopts hydrothermal method, electrochemical deposition method, magnetron sputtering method, sol-gel method, etc., which are not suitable for large-scale preparation of large-area electrochromic films. It can be seen that although nickel oxide has achieved remarkable results in laboratory research, its preparation process and cost issues are still the main obstacles to its large-scale application. Therefore, the development of a simple, efficient and cost-controlled method for preparing nickel oxide electrochromic films has important practical application value and broad market prospects. Summary of the invention

[0004] The present invention proposes a carbon-nitrogen co-doped NiO electrochromic film and a smart window and a preparation method thereof, so as to solve the problems of high difficulty in material synthesis, high synthesis cost, complex film forming equipment and poor film uniformity in the prior art.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] One of the technical solutions of the present invention:

[0007] A method for preparing a carbon-nitrogen co-doped NiO electrochromic film comprises the following steps:

[0008] The nickel salt is dissolved in anhydrous ethanol, ethanolamine is added, and the mixture is stirred to form a nickel salt solution, which is then sprayed on the surface of a substrate and cured to obtain a carbon-nitrogen co-doped NiO electrochromic film.

[0009] In the present invention, the role of ethanolamine is as follows:

[0010] 1. Chelating agent effect

[0011] Ethanolamine has an amino group (-NH 2 ) and hydroxyl (-OH), which enables it to react with nickel ions (Ni 2+ ) to form a coordination complex. Through chelation, ethanolamine can stabilize the dispersion of nickel ions in the solution, preventing the nickel ions from precipitating prematurely or forming uneven particles. This helps to maintain the uniformity and stability of the solution, thereby obtaining a more uniform nickel oxide film during the subsequent spraying and film formation process.

[0012] 2. Adjust the pH value of the solution

[0013] Ethanolamine is a weak alkaline substance, which can partially neutralize the acidity in the solution and adjust the pH value of the solution. The appropriate pH value can control the hydrolysis rate of the nickel salt and the formation conditions of nickel oxide, thereby helping to form the desired nickel oxide (NiO) structure and performance.

[0014] 3. Increase the viscosity of the solution

[0015] The addition of ethanolamine can increase the viscosity of the solution, which is very important for the spraying process. Appropriate viscosity helps to form a uniform solution layer and prevents the droplets from flowing too fast during the spraying process, thereby achieving uniform film coverage.

[0016] Preferably, in the method for preparing the carbon-nitrogen co-doped NiO electrochromic thin film, the concentration of the nickel salt solution is 0.05-0.5 mol / L.

[0017] Preferably, in the method for preparing the carbon-nitrogen co-doped NiO electrochromic film, the substrate is conductive glass, more preferably ITO conductive glass.

[0018] Preferably, in the method for preparing the carbon-nitrogen co-doped NiO electrochromic film, the nickel salt is a soluble nickel salt, including nickel acetate, nickel chloride, nickel nitrate or nickel sulfate.

[0019] Preferably, in the method for preparing the carbon-nitrogen co-doped NiO electrochromic film, the ratio of the volume of the ethanolamine to the amount of substance of the nickel salt is (50-1000) mL: (1-10) mol.

[0020] The effect of the ratio of the volume of ethanolamine to the amount of nickel salt on the film properties is as follows:

[0021] 1. Crystallinity and structure of the film

[0022] Increased proportion of ethanolamine: Ethanolamine is a chelating agent that can form a stable complex with nickel ions, which affects the crystallinity of nickel oxide (NiO) in the film. Higher ethanolamine content may result in a more uniform film structure, but may also reduce the size of the crystallites, resulting in reduced film crystallinity.

[0023] Higher nickel acetate ratio: There will be more nickel sources to supply the film growth, which may lead to higher crystallinity, but if ethanolamine is insufficient, it may cause uneven distribution of nickel ions during deposition, resulting in increased film defects.

[0024] 2. Electrochromic properties of thin films

[0025] Moderate ratio of ethanolamine: A proper amount of ethanolamine can ensure uniform nickel source deposition and form a dense NiO film, which helps to improve the electrochromic efficiency and cycle stability of the film.

[0026] Too high a proportion of ethanolamine may lead to excessive complexation of nickel ions during the deposition process, reduce the effective deposition amount of NiO, and the electrochromic properties of the film may be reduced as a result.

[0027] 3. Surface morphology of the film

[0028] Ethanolamine ratio affects surface smoothness: Ethanolamine can regulate the viscosity and complexation state of the solution, which directly affects the leveling and adhesion of the film on the substrate. Too much ethanolamine may make the film surface smoother, but too little may cause uneven film surface or even cracks.

[0029] 4. Chemical composition and doping effect

[0030] Carbon and nitrogen doping effect: Ethanolamine contains nitrogen and carbon sources, which can introduce carbon and nitrogen elements into the NiO lattice during high-temperature heat treatment. Different proportions may affect the doping degree, thereby changing the optical band gap, conductivity and other properties of the film.

[0031] 5. Conductivity and electrochemical properties of films

[0032] Uniformity of carbon and nitrogen doping: When the ratio of ethanolamine is appropriate, the doping may be more uniform, which helps to improve the conductivity and electrochemical properties of the film. If the ratio is unbalanced, uneven doping may lead to reduced film conductivity and affect the response speed and cycle stability of the electrochromic.

[0033] Preferably, in the method for preparing the carbon-nitrogen co-doped NiO electrochromic film, the curing is a heat treatment, and the temperature of the heat treatment is 150-300°C and the time is 0.5-1.5h. The heat treatment temperature determines the composition change of the solute in the solution. As the temperature increases, the solute gradually changes from an organic mixture at the beginning to an inorganic substance, and the color change performance shows a process of first increasing and then decreasing.

[0034] The second technical solution of the present invention:

[0035] The invention provides a carbon-nitrogen co-doped NiO electrochromic film obtained according to the preparation method.

[0036] The third technical solution of the present invention:

[0037] The present invention also provides a carbon-nitrogen co-doped NiO electrochromic glass, the surface of which is coated with a carbon-nitrogen co-doped NiO electrochromic film.

[0038] The fourth technical solution of the present invention:

[0039] The present invention also provides a carbon-nitrogen co-doped NiO electrochromic smart window, which is prepared from the carbon-nitrogen co-doped NiO electrochromic film or the carbon-nitrogen co-doped NiO electrochromic glass.

[0040] The fifth technical solution of the present invention:

[0041] The present invention also provides a method for preparing the carbon-nitrogen co-doped NiO electrochromic smart window. When the carbon-nitrogen co-doped NiO electrochromic thin film is prepared, the preparation method comprises the following steps: coating the carbon-nitrogen co-doped NiO electrochromic thin film on the surface of conductive glass to obtain glass coated with the carbon-nitrogen co-doped NiO electrochromic thin film, overlapping the glass with another conductive glass, injecting electrolyte between the glass coated with the carbon-nitrogen co-doped NiO electrochromic thin film and the conductive glass, sealing, and connecting an external circuit to obtain the carbon-nitrogen co-doped NiO electrochromic smart window;

[0042] When prepared from the above-mentioned carbon-nitrogen co-doped NiO electrochromic glass, the preparation method includes the following steps: overlapping the carbon-nitrogen co-doped NiO electrochromic glass and conductive glass, injecting electrolyte between the carbon-nitrogen co-doped NiO electrochromic glass and the conductive glass, sealing, connecting an external circuit, and obtaining the carbon-nitrogen co-doped NiO electrochromic smart window.

[0043] Preferably, in the method for preparing the carbon-nitrogen co-doped NiO electrochromic smart window, the conductive glass is ITO conductive glass.

[0044] Preferably, in the method for preparing the carbon-nitrogen co-doped NiO electrochromic smart window, the carbon-nitrogen co-doped NiO electrochromic film has a thickness of 50 to 500 nm, more preferably 150 to 350 nm. In the present invention, the main factor leading to different film thicknesses is the spraying amount.

[0045] Preferably, in the method for preparing the carbon-nitrogen co-doped NiO electrochromic smart window, the electrolyte is a potassium hydroxide (KOH) solution with a concentration of 0.1 to 1.0 mol / L.

[0046] Technical solution six of the present invention:

[0047] The present invention also provides the use of the carbon-nitrogen co-doped NiO electrochromic film or the carbon-nitrogen co-doped NiO electrochromic glass in an electrochromic smart window.

[0048] When a voltage is applied to the electrochromic smart window, the color changes from colorless and transparent to brown-black.

[0049] Compared with the prior art, the present invention has the following advantages and technical effects:

[0050] 1. Since carbon-nitrogen co-doped NiO can improve the conductivity of the material, the NiO film has higher coloring efficiency, faster response speed and good light regulation performance. At the same time, the amorphous crystal structure can avoid the structural collapse caused by volume expansion, thereby increasing the cycle stability to more than 5,000 times, which is suitable for fields such as building energy-saving windows and has broad market prospects and application potential.

[0051] 2. The present invention adopts a simple and easy-to-operate spraying method to prepare a carbon-nitrogen co-doped NiO film on an ITO conductive glass, and the target product can be obtained by appropriate heat treatment. The entire preparation process does not require complex equipment and processes, which reduces the production cost and technical threshold, and is suitable for large-scale, large-area production and application. The film prepared at the same time is sprayed out by compressed air and immediately attached to the glass surface, and at the same time, the solvent in the solution is volatilized at a suitable temperature, and in a spraying operation, it undergoes repeated spraying, attachment, and solvent solute separation and volatilization at intervals, regularly, and relatively evenly. The solute has a strong binding force with the glass, and then undergoes a long-term heat treatment at a suitable temperature, which further improves the adhesion of the film. Therefore, the film is not easy to fall off during long-term use, ensuring the long-term stability and reliability of the smart window.

[0052] 3. The present invention uses environmentally friendly solvents such as anhydrous ethanol and ethanolamine, which reduces the emission of harmful gases compared to traditional chemical vapor deposition methods. In addition, raw materials such as nickel acetate, nickel chloride, nickel nitrate and nickel sulfate are relatively cheap, further reducing production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0054] Figure 1 This is a real picture of the coloring / fading of the carbon-nitrogen co-doped nickel oxide electrochromic smart window of Example 1;

[0055] Figure 2 1 is a SEM image of the carbon-nitrogen co-doped nickel oxide electrochromic thin film glass of Example 1, wherein a is a SEM image of the surface of the carbon-nitrogen co-doped nickel oxide electrochromic thin film glass; b is a SEM image of the cross section of the carbon-nitrogen co-doped nickel oxide electrochromic thin film glass;

[0056] Figure 3 TEM image of the carbon-nitrogen co-doped nickel oxide electrochromic film of Example 1;

[0057] Figure 4 is an electron diffraction pattern of the carbon-nitrogen co-doped nickel oxide electrochromic thin film of Example 1;

[0058] Figure 5 : is the energy spectrum element analysis diagram of the carbon-nitrogen co-doped nickel oxide electrochromic thin film of Example 1;

[0059] Figure 6 This is a light transmittance diagram of the carbon-nitrogen co-doped NiO electrochromic smart window when it is on / off in Example 1;

[0060] Figure 7 This is a response time diagram of the carbon-nitrogen co-doped NiO electrochromic smart window of Example 1;

[0061] Figure 8 This is a light transmittance diagram of the carbon-nitrogen co-doped NiO electrochromic smart window when it is on / off in Example 2;

[0062] Fig. 9 This is a response time diagram of the carbon-nitrogen co-doped NiO electrochromic smart window of Example 2;

[0063] Fig.10 This is a light transmittance diagram of the carbon-nitrogen co-doped NiO electrochromic smart window during coloring / fading of Comparative Example 3;

[0064] Fig.11This is the response time diagram of the carbon-nitrogen co-doped NiO electrochromic smart window of Comparative Example 3. DETAILED DESCRIPTION

[0065] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0066] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0067] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0068] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0069] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0070] Unless otherwise specified, the room temperature in the present invention is 25±2°C.

[0071] All raw materials used in the examples of the present invention are commercially available.

[0072] The technical solution of the present invention is further illustrated by the following embodiments.

[0073] Example 1

[0074] This embodiment provides a carbon-nitrogen co-doped NiO electrochromic film and a smart window, and the preparation method thereof is as follows:

[0075] (1) Weigh 0.497 g (3 mmol) of nickel acetate and dissolve it in 20 mL of anhydrous ethanol, add 120 μL of ethanolamine, mix and stir evenly to form a green clear transparent solution (i.e., nickel salt solution). The concentration of the nickel salt solution in this embodiment is 0.15 mol / L;

[0076] (2) Spray 2 mL of the nickel salt solution onto the surface of a cleaned ITO conductive glass (6 cm*7 cm, the same below), and heat treat at 250° C. for 1.5 hours to obtain a carbon-nitrogen co-doped NiO electrochromic thin film glass (in this step, the carbon-nitrogen co-doped NiO electrochromic thin film is torn off from the ITO conductive glass to obtain the carbon-nitrogen co-doped NiO electrochromic thin film);

[0077] (3) Dissolve potassium hydroxide (KOH) in 40 mL of water to obtain a 0.1 mol / L electrolyte;

[0078] (4) stacking a carbon-nitrogen co-doped NiO electrochromic thin film glass and another ITO conductive glass, injecting the above electrolyte between the carbon-nitrogen co-doped NiO electrochromic thin film glass and the ITO conductive glass, sealing, and connecting an external circuit to obtain a carbon-nitrogen co-doped NiO electrochromic smart window.

[0079] The carbon-nitrogen co-doped NiO electrochromic smart window prepared in this embodiment was subjected to a simulation test, and the actual coloring / fading picture is shown in FIG. Figure 1 As shown. Figure 1 It can be seen that at room temperature, the smart window is highly transparent (corresponding to the first on the left); when a voltage of 1V is applied, the smart window is tinted and appears brown-black (corresponding to the fourth on the left); when a voltage of -0.5V is applied, the smart window fades and returns to a highly transparent state (corresponding to the second on the left). After 3,000 cycles, it can still return to a highly transparent state (corresponding to the third on the left).

[0080] The glass with carbon-nitrogen co-doped NiO electrochromic thin film prepared in this example was subjected to SEM test, and the results are as follows: Figure 2 As shown. Figure 2 It can be seen that the NiO nanofilm is sprayed evenly on the surface of the conductive glass, and the particles are regular spheres of 30 to 80 nm. From the cross section, it can be seen that the film thickness is about 50 to 150 nm and is tightly bonded to the substrate.

[0081] The glass with carbon-nitrogen co-doped NiO electrochromic thin film prepared in this embodiment was subjected to TEM test, electron diffraction and energy spectrum analysis. The results are as follows: Figure 3 , 4 , 5. Figure 3 It can be seen that NiO nanoparticles are in the form of flakes; Figure 4It can be seen that NiO nanoparticles are not crystallized, and their amorphous crystal structure can avoid the structural collapse caused by volume expansion, thereby improving the cycle stability; Figure 5 It can be seen that NiO nanoparticles contain not only Ni and O elements, but also C and N elements.

[0082] Voltage was applied to the carbon-nitrogen co-doped NiO electrochromic smart window prepared in this example, and the light transmittance was measured during fading. The results are as follows: Figure 6 As shown. Figure 6 It can be seen that the modulation amplitude of the visible light transmittance at 500 nm (ie, the spectrum modulation amplitude in Table 1) reaches 57.7%, and the modulation amplitude can still be maintained above 80% after 5000 cycles.

[0083] The carbon-nitrogen co-doped NiO electrochromic smart window prepared in this embodiment was subjected to a cyclic test by coloring at +1V for 30s and fading at -0.5V for 30s during the electrochromic process, and a curve of the transmittance changing with time was measured. The results are shown in FIG. Figure 7 As shown. Figure 7 It can be seen that in each electrochromic process (one coloring and fading), the coloring time is 11 s and the fading time is 7 s.

[0084] Example 2

[0085] This embodiment provides a carbon-nitrogen co-doped NiO electrochromic smart window, and its preparation method is the same as that of Example 1, except that the heat treatment temperature is changed to 150°C.

[0086] Voltage was applied to the carbon-nitrogen co-doped NiO electrochromic smart window prepared in this example, and the light transmittance was measured during fading. The results are as follows: Figure 8 As shown. Figure 8 It can be seen that the modulation amplitude of the visible light transmittance at 500 nm is 27.3%, and the modulation amplitude remains above 80% after 3000 cycles.

[0087] The carbon-nitrogen co-doped NiO electrochromic smart window prepared in this embodiment was subjected to a cyclic test by coloring at +1V for 30s and fading at -0.5V for 30s during the electrochromic process, and a curve of the transmittance changing with time was measured. The results are shown in FIG. Fig. 9 As shown. Fig. 9 It can be seen that in each electrochromic process (one coloring and fading), the coloring time is 7s and the fading time is 7s.

[0088] Example 3

[0089] This embodiment provides a carbon-nitrogen co-doped NiO electrochromic smart window, and its preparation method is the same as that of Example 1, except that the heat treatment temperature is changed to 200°C.

[0090] Voltage was applied to the carbon-nitrogen co-doped NiO electrochromic smart window prepared in this embodiment, and the light transmittance was measured during fading. The modulation amplitude of the visible light transmittance at 500nm was 37.7%, and the modulation amplitude was still maintained above 80% after 2500 cycles.

[0091] The carbon-nitrogen co-doped NiO electrochromic smart window prepared in this embodiment was subjected to a cyclic test during the electrochromic process by coloring at +1V for 30s and fading at -0.5V for 30s, and a curve graph of the transmittance changing with time was measured. In each electrochromic process (one coloring and fading), the coloring time was 6.0s and the fading time was 19.0s.

[0092] Example 4

[0093] This embodiment provides a carbon-nitrogen co-doped NiO electrochromic smart window, and its preparation method is the same as that of Example 1, except that both the heat treatment temperature and the heat treatment time are changed, so that the heat treatment temperature is 150° C. and the heat treatment time is 30 minutes.

[0094] Voltage was applied to the carbon-nitrogen co-doped NiO electrochromic smart window prepared in this embodiment, and the light transmittance was measured during fading. The modulation amplitude of the visible light transmittance at 500nm was 23.7%, and the modulation amplitude was still maintained above 80% after 1000 cycles.

[0095] The carbon-nitrogen co-doped NiO electrochromic smart window prepared in this embodiment was subjected to a cyclic test during the electrochromic process by coloring at +1V for 30s and fading at -0.5V for 30s, and a curve graph of the transmittance changing with time was measured. In each electrochromic process (one coloring and fading), the coloring time was 5.5s and the fading time was 14.1s.

[0096] Example 5

[0097] This embodiment provides a carbon-nitrogen co-doped NiO electrochromic smart window, and its preparation method is the same as that of comparative example 1, except that both the heat treatment temperature and the heat treatment time are changed, so that the heat treatment temperature is 300° C. and the heat treatment time is 30 minutes.

[0098] Voltage was applied to the carbon-nitrogen co-doped NiO electrochromic smart window prepared in this embodiment, and the light transmittance was measured during fading. The modulation amplitude of the visible light transmittance at 500nm was 46.4%, and the modulation amplitude was still maintained above 80% after 2000 cycles.

[0099] The carbon-nitrogen co-doped NiO electrochromic smart window prepared in this embodiment was subjected to a cyclic test during the electrochromic process by coloring at +1V for 30s and fading at -0.5V for 30s, and a curve graph of the transmittance changing with time was measured. In each electrochromic process (one coloring and fading), the coloring time was 7.9s and the fading time was 22.1s.

[0100] Example 6

[0101] (1) 1.296 g (10 mmol) of nickel chloride was weighed and dissolved in 20 mL of anhydrous ethanol, and 500 μL of ethanolamine was added and mixed and stirred to form a green clear and transparent solution (i.e., a nickel salt solution). In this embodiment, the concentration of the nickel salt solution is 0.5 mol / L;

[0102] (2) Spray 2 mL of the above solution onto the cleaned surface of ITO conductive glass, and heat treat at 250° C. for 1.5 hours to obtain carbon-nitrogen co-doped NiO electrochromic thin film glass;

[0103] (3) Dissolve KOH in 40 mL of water to obtain a 0.5 mol / L electrolyte;

[0104] (4) Stacking the carbon-nitrogen co-doped NiO electrochromic thin film glass with another ITO conductive glass, injecting the above electrolyte between the carbon-nitrogen co-doped NiO electrochromic thin film glass and the conductive glass, sealing, and connecting an external circuit to obtain a carbon-nitrogen co-doped NiO electrochromic smart window.

[0105] Voltage was applied to the carbon-nitrogen co-doped NiO electrochromic smart window prepared in this embodiment, and the light transmittance was measured during fading. The modulation amplitude of the visible light transmittance at 500nm was 13.3%, and the modulation amplitude was still maintained above 80% after 1000 cycles.

[0106] The carbon-nitrogen co-doped NiO electrochromic smart window prepared in this embodiment was subjected to a cyclic test during the electrochromic process by coloring at +1V for 30s and fading at -0.5V for 30s, and a curve graph of the transmittance changing with time was measured. In each electrochromic process (one coloring and fading), the coloring time was 18.4s and the fading time was 31.1s.

[0107] Example 7

[0108] (1) Weigh 0.183 g (1 mmol) of nickel nitrate and dissolve it in 20 mL of anhydrous ethanol, add 100 μL of ethanolamine, mix and stir evenly to form a green clear and transparent solution (i.e., nickel salt solution). The concentration of the nickel salt solution in this embodiment is 0.05 mol / L;

[0109] (2) Spray 2 mL of the above solution onto the cleaned surface of ITO conductive glass, and heat treat at 250° C. for 1.5 hours to obtain carbon-nitrogen co-doped NiO electrochromic thin film glass;

[0110] (3) Dissolve KOH in 40 mL of water to obtain a 1.0 mol / L electrolyte;

[0111] (4) Stacking the carbon-nitrogen co-doped NiO electrochromic thin film glass with another ITO conductive glass, injecting the above electrolyte between the carbon-nitrogen co-doped NiO electrochromic thin film glass and the conductive glass, sealing, and connecting an external circuit to obtain a carbon-nitrogen co-doped NiO electrochromic smart window.

[0112] Voltage was applied to the carbon-nitrogen co-doped NiO electrochromic smart window prepared in this embodiment, and the light transmittance was measured during fading. The modulation amplitude of the visible light transmittance at 500nm was 35.9%, and the modulation amplitude was still maintained above 80% after 1000 cycles.

[0113] The carbon-nitrogen co-doped NiO electrochromic smart window prepared in this embodiment was subjected to a cyclic test by coloring at +1V for 30s and fading at -0.5V for 30s during the electrochromic process, and a curve graph of the transmittance changing with time was measured. In each electrochromic process (one coloring and fading), the coloring time was 16.9s and the fading time was 24.1s.

[0114] Example 8

[0115] (1) Weigh 0.774 g (5 mmol) of nickel sulfate and dissolve it in 20 mL of anhydrous ethanol, add 50 μL of ethanolamine, mix and stir evenly to form a green clear transparent solution (i.e., nickel salt solution). The concentration of the nickel salt solution in this embodiment is 0.25 mol / L;

[0116] (2) Spray 2 mL of the above solution onto the cleaned surface of ITO conductive glass, and heat treat at 250° C. for 1.5 hours to obtain carbon-nitrogen co-doped NiO electrochromic thin film glass;

[0117] (3) Dissolve KOH in 40 mL of water to obtain a 0.5 mol / L electrolyte;

[0118] (4) Stacking the carbon-nitrogen co-doped NiO electrochromic thin film glass with another ITO conductive glass, injecting the above electrolyte between the carbon-nitrogen co-doped NiO electrochromic thin film glass and the conductive glass, sealing, and connecting an external circuit to obtain a carbon-nitrogen co-doped NiO electrochromic smart window.

[0119] Voltage was applied to the carbon-nitrogen co-doped NiO electrochromic smart window prepared in this embodiment, and the light transmittance was measured during fading. The modulation amplitude of the visible light transmittance at 500 nm was 25.0%, and the modulation amplitude was still maintained above 80% after 1500 cycles.

[0120] The carbon-nitrogen co-doped NiO electrochromic smart window prepared in this embodiment was subjected to a cyclic test during the electrochromic process by coloring at +1V for 30s and fading at -0.5V for 30s, and a curve graph of the transmittance changing with time was measured. In each electrochromic process (one coloring and fading), the coloring time was 18.6s and the fading time was 25.7s.

[0121] Comparative Example 1

[0122] This comparative example provides a carbon-nitrogen co-doped NiO electrochromic smart window, and its preparation method is the same as that of Example 1, except that the KOH electrolyte is replaced by dissolved LiClO 4 of polycarbonate solution to a concentration of 1 mol / L.

[0123] When voltage was applied to the carbon-nitrogen co-doped NiO electrochromic smart window prepared in this comparative example, it was found that it did not change color.

[0124] Reason for performance degradation: OH - It is easier to embed and remove, and the process is relatively rapid. It is relatively easy to observe color change in a short time, and NiO usually exhibits good electrochromic performance in alkaline electrolytes; while Li + The embedding and extraction process is slower, and the embedding / extraction process is not sufficient or strong enough to cause a significant redox reaction of the NiO film, thereby failing to effectively change the optical properties of the material.

[0125] Comparative Example 2

[0126] This comparative example provides a carbon-nitrogen co-doped NiO electrochromic smart window, and its preparation method is the same as that of Example 1, except that the heat treatment time is changed to 60 minutes.

[0127] Voltage was applied to the carbon-nitrogen co-doped NiO electrochromic smart window prepared in this comparative example, and the light transmittance during fading was measured. The modulation amplitude of the visible light transmittance at 500 nm was 19.1%.

[0128] The carbon-nitrogen co-doped NiO electrochromic smart window prepared in this comparative example was subjected to a cyclic test by coloring at +1V for 30s and fading at -0.5V for 30s during the electrochromic process, and a curve graph of the transmittance changing with time was measured. In each electrochromic process (one coloring and fading), the coloring time was 8.0s and the fading time was 14.0s.

[0129] Reasons for performance degradation: short heat treatment time, less color-changing substance conversion, reduced color-changing activity, and reduced modulation amplitude.

[0130] Comparative Example 3

[0131] This comparative example provides a carbon-nitrogen co-doped NiO electrochromic smart window, and its preparation method is the same as that of comparative example 1, except that the heat treatment temperature is changed to 350°C.

[0132] Voltage was applied to the carbon-nitrogen co-doped NiO electrochromic smart window prepared in this comparative example, and the light transmittance was measured during fading. The results are as follows: Fig.10 As shown. Fig.10 It can be seen that the modulation amplitude of the visible light transmittance at 500 nm is 15.5%, and the modulation amplitude remains at about 80% after 800 cycles.

[0133] The carbon-nitrogen co-doped NiO electrochromic smart window prepared in this comparative example was subjected to a cyclic test by coloring at +1V for 10s and fading at -0.5V for 20s during the electrochromic process, and a curve of the transmittance changing with time was measured. The results are shown in FIG. Fig.11 As shown. Fig.11 It can be seen that in each electrochromic process (one coloring and fading), the coloring time is 6.0 s and the fading time is 11.0 s.

[0134] Reasons for performance degradation: The heat treatment temperature is high, the color-changing substance is converted into NiO, the color-changing activity is reduced, and the modulation amplitude is reduced.

[0135] Comparative Example 4

[0136] This comparative example provides a carbon-nitrogen co-doped NiO electrochromic smart window, and its preparation method is the same as that of comparative example 1, except that both the heat treatment temperature and the heat treatment time are changed, so that the heat treatment temperature is 300°C and the heat treatment time is 60 minutes.

[0137] Voltage was applied to the carbon-nitrogen co-doped NiO electrochromic smart window prepared in this comparative example, and the light transmittance was measured during fading. The modulation amplitude of the visible light transmittance at 500nm was 8.9%, and the modulation amplitude remained at about 80% after 700 cycles.

[0138] The carbon-nitrogen co-doped NiO electrochromic smart window prepared in this comparative example was subjected to a cyclic test during the electrochromic process by coloring at +1V for 30s and fading at -0.5V for 30s, and a curve graph of the transmittance changing with time was measured. In each electrochromic process (one coloring and fading), the coloring time was 9.2s and the fading time was 16.6s.

[0139] Reasons for performance degradation: high heat treatment temperature, increased content of inactive substances, reduced color change activity, and reduced spectral modulation amplitude.

[0140] Comparative Example 5

[0141] This comparative example provides a carbon-nitrogen co-doped NiO electrochromic smart window, and its preparation method is the same as that of comparative example 1, except that both the heat treatment temperature and the heat treatment time are changed, so that the heat treatment temperature is 300°C and the heat treatment time is 90 minutes.

[0142] Voltage was applied to the carbon-nitrogen co-doped NiO electrochromic smart window prepared in this comparative example, and the light transmittance was measured during fading. The modulation amplitude of the visible light transmittance at 500nm was 5.4%, and the modulation amplitude remained at about 80% after 500 cycles.

[0143] The carbon-nitrogen co-doped NiO electrochromic smart window prepared in this comparative example was subjected to a cyclic test during the electrochromic process by coloring at +1V for 30s and fading at -0.5V for 30s, and a curve graph of the transmittance changing with time was measured. In each electrochromic process (one coloring and fading), the coloring time was 7.3s and the fading time was 12.4s.

[0144] Reasons for performance degradation: high heat treatment temperature, increased content of inactive substances, reduced color change activity, and reduced spectral modulation amplitude.

[0145] Comparative Example 6

[0146] This comparative example provides a carbon-nitrogen co-doped NiO electrochromic smart window, the preparation method of which is the same as that of comparative example 1, except that the amount of the spray solution is changed so that the volume of the spray solution is 1 mL and the film thickness is about 50 to 150 nm. No color change occurs after voltage is applied.

[0147] Reasons for performance degradation: The volume of the sprayed solution is too small, resulting in too little active substance in the film on the glass surface after heat treatment. After power is turned on, the modulation amplitude is greatly reduced and no obvious color change can occur.

[0148] Comparative Example 7

[0149] This comparative example provides a carbon-nitrogen co-doped NiO electrochromic smart window, and its preparation method is the same as that of comparative example 1, except that the amount of the spraying solution is changed so that the volume of the spraying solution is 3 mL and the film thickness is about 300 to 500 nm.

[0150] Voltage was applied to the carbon-nitrogen co-doped NiO electrochromic smart window prepared in this comparative example, and the light transmittance was measured during fading. The modulation amplitude of the visible light transmittance at 500 nm was 4.5%, and the modulation amplitude remained at 60% after 500 cycles.

[0151] The carbon-nitrogen co-doped NiO electrochromic smart window prepared in this comparative example was subjected to a cyclic test by coloring at +1V for 30s and fading at -0.5V for 30s during the electrochromic process, and a curve graph of the transmittance changing with time was measured. In each electrochromic process (one coloring and fading), the coloring time was 8.7s and the fading time was 20.5s.

[0152] Reasons for performance degradation: The film is too thick, which hinders the embedding and extraction of ions, and the migration path of charges and ions becomes longer, resulting in a lower response speed of electrochromic and failure to achieve the effect of rapid color change; and a film that is too thick may absorb too much light during the color change process, resulting in a decrease in the optical difference between the transparent and colored states, thereby reducing the spectral modulation amplitude.

[0153] Comparative Example 8

[0154] This embodiment provides a carbon-nitrogen co-doped NiO electrochromic smart window, and its preparation method is the same as that of Example 1, except that ethanolamine is not added.

[0155] Voltage was applied to the carbon-nitrogen co-doped NiO electrochromic smart window prepared in this comparative example, and the light transmittance was measured during fading. The modulation amplitude of the visible light transmittance at 500nm was 4.4%, and the modulation amplitude remained at 60% after 200 cycles.

[0156] The carbon-nitrogen co-doped NiO electrochromic smart window prepared in this comparative example was subjected to a cyclic test by coloring at +1V for 30s and fading at -0.5V for 30s during the electrochromic process, and a curve graph of the transmittance changing with time was measured. In each electrochromic process (one coloring and fading), the coloring time was 7.0s and the fading time was 18.0s.

[0157] Reasons for performance degradation: lack of ethanolamine nickel ions (Ni 2+ ) may aggregate more easily in the solution, resulting in uneven, rough or porous areas in the film during the deposition process; and without the addition of ethanolamine, the amount of carbon and nitrogen doping in the film may be greatly reduced or completely absent, resulting in reduced electrochromic activity, response speed and stability of the film.

[0158] Voltage was applied to the carbon-nitrogen co-doped NiO electrochromic smart windows prepared in Examples 1 to 5 and Comparative Examples 2 to 7, and the light transmittance during coloring / fading was measured. The results are shown in Table 1.

[0159] Table 1 Test results of light transmittance of carbon-nitrogen co-doped NiO electrochromic smart window at 500nm

[0160]

[0161] Note: In Table 1, “volume of solution” refers to the spraying volume of nickel salt solution.

[0162] As shown in Table 1, when KOH aqueous solution is used as the electrolyte, the spectral modulation amplitude fluctuates in a wide range. The best conditions are a spray solution volume of 2 mL, a heat treatment temperature of 250 ° C, and a heat treatment time of 90 min. The spectral modulation amplitude can reach up to 57.7%, which can effectively regulate the visible light transmittance in summer. In the coloring / fading state, it can meet the requirements of light transmission and shading, and play a role in lighting, adjusting indoor temperature or protecting privacy. In addition, the device requires a small voltage (0.6 V) for electrochromism, which can effectively simplify the structural components of the smart window, save energy, and has high stability.

[0163] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A method for preparing a carbon-nitrogen co-doped NiO electrochromic film, It is characterized in that The following steps are involved: The nickel salt is dissolved in anhydrous ethanol, ethanolamine is added, and the mixture is stirred to form a nickel salt solution, which is then sprayed on the surface of a substrate and cured to obtain a carbon-nitrogen co-doped NiO electrochromic film.

2. The method for preparing the carbon-nitrogen co-doped NiO electrochromic thin film according to claim 1, It is characterized in that The concentration of the nickel salt solution is 0.05-0.5 mol / L.

3. The method for preparing the carbon-nitrogen co-doped NiO electrochromic thin film according to claim 1, It is characterized in that The ratio of the volume of the ethanolamine to the amount of substance of the nickel salt is (50-1000) mL: (1-10) mol.

4. The method for preparing the carbon-nitrogen co-doped NiO electrochromic thin film according to claim 1, It is characterized in that The curing is a heat treatment, the temperature of the heat treatment is 150-300° C., and the time is 0.5-1.5 h.

5. A carbon-nitrogen co-doped NiO electrochromic film, It is characterized in that Obtained according to the preparation method according to any one of claims 1 to 4.

6. A carbon-nitrogen co-doped NiO electrochromic glass, It is characterized in that The surface contains the carbon-nitrogen co-doped NiO electrochromic film as claimed in claim 5.

7. A carbon-nitrogen co-doped NiO electrochromic smart window, It is characterized in that The electrochromic film is prepared from the carbon-nitrogen co-doped NiO electrochromic film as described in claim 5 or the carbon-nitrogen co-doped NiO electrochromic glass as described in claim 6.

8. Use of the carbon-nitrogen co-doped NiO electrochromic film according to claim 5 or the carbon-nitrogen co-doped NiO electrochromic glass according to claim 6 in electrochromic smart windows.

9. The method for preparing the carbon-nitrogen co-doped NiO electrochromic smart window according to claim 7, It is characterized in that When prepared by the carbon-nitrogen co-doped NiO electrochromic film according to claim 5, the preparation method comprises the following steps: coating the carbon-nitrogen co-doped NiO electrochromic film on the surface of conductive glass to obtain glass coated with the carbon-nitrogen co-doped NiO electrochromic film, overlapping it with another conductive glass, injecting electrolyte between the glass coated with the carbon-nitrogen co-doped NiO electrochromic film and the conductive glass, sealing, connecting an external circuit, and obtaining the carbon-nitrogen co-doped NiO electrochromic smart window; When prepared from the carbon-nitrogen co-doped NiO electrochromic glass as described in claim 6, the preparation method comprises the following steps: overlapping the carbon-nitrogen co-doped NiO electrochromic glass and conductive glass, injecting electrolyte between the carbon-nitrogen co-doped NiO electrochromic glass and the conductive glass, sealing, connecting an external circuit, and obtaining the carbon-nitrogen co-doped NiO electrochromic smart window.

10. The method for preparing the carbon-nitrogen co-doped NiO electrochromic smart window according to claim 9, It is characterized in that The thickness of the carbon-nitrogen co-doped NiO electrochromic film is 50-500 nm.

Citation Information

Patent Citations

  • Intelligent glass capable of conducting electrochromism, electrochemical energy storage and electronic equipment driving

    CN104111568A

  • NiO composite film, quantum dot light-emitting device and the preparation and application of the same

    CN107240624A