Preparation method and application of high-volume-density prebaked anode
By using a modified filler in the prebaked anode, the interaction between calcined coke and coal asphalt is enhanced, the problem of low volume density of traditional anodes is solved, the high volume density and pressure resistance strength are improved, and aluminum electrolytic production is improved efficiency and product quality.
Patent Information
- Application Number
- CN202411119794.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-15
AI Technical Summary
The bonding strength of calcined coke and coal asphalt in traditional prebaked anodes is limited, resulting in a low volume density, affecting the conductivity and heat resistance, and thus reducing the mechanical strength and service life of the anode.
Using a modified filler, the interaction of coal asphalt is enhanced through alkenylation of graphene quantum dots and grafting of sulfur polymers, combined with calcined coke and modified asphalt, and the anode is improved through gradient heating calcination and vibration forming processes. volume density.
A prebaked anode with a high volume density is achieved, with a volume density of 1.95g·cm-3, which reduces porosity, improves pressure resistance and reduces resistivity, significantly improving the efficiency and product quality of aluminum electrolytic production.
Smart Images

Figure BDA0004994707070000081 
Figure BDA0004994707070000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum electrolysis, and in particular to a preparation method of a prebaked anode with high volume density and application thereof. Background Art
[0002] Prebaked anode is an important component in the aluminum electrolysis process, and its performance directly affects the electrolysis efficiency and product quality of aluminum. Traditional prebaked anode is mainly composed of a mixture of calcined coke and coal tar. However, there is a significant problem with the current technology, that is, the bonding strength between calcined coke and coal tar is limited. During the bonding process, the insufficient interfacial interaction will lead to a low volume density of the prebaked anode, which in turn affects its electrical conductivity and heat resistance. The lower volume density not only reduces the mechanical strength of the anode, but may also cause the disintegration of the anode and reduce its service life during the electrolysis process. This problem poses a challenge to energy consumption and production efficiency in the aluminum electrolysis industry.
[0003] Patent technical document CN201710003876.5 discloses a prebaked anode for aluminum electrolysis and its production process, the raw materials of which include, by weight percentage: 82-86% of batching components and 14%-18% of adhesive, wherein the batching components include, by weight percentage, 80%-84% of calcined petroleum coke, 14%-16% of residual anode with an ash content of less than 1%, and 2%-4% of cathode milling flour produced during the processing of cathodes for aluminum electrolysis. The adhesive includes coal tar and additives, and the additives include one or more of epoxy resin, phenolic resin, furfural resin, and furan resin. The invention uses a resin and coal tar compound as an adhesive to increase the volume density of the prebaked anode for aluminum electrolysis, but the distribution and roasting process of the resin may lead to uneven bonding strength, thereby affecting the mechanical strength and conductivity of the anode. Summary of the invention
[0004] In view of this, the purpose of the present invention is to propose a method for preparing a prebaked anode with high volume density and its application, so as to solve the problem of limited bonding strength between calcined coke and coal tar pitch, resulting in low volume density of the prebaked anode.
[0005] Based on the above purpose, the present invention provides a method for preparing a prebaked anode with high volume density, comprising the following steps:
[0006] (1) Mixing: mixing calcined coke and coal tar pitch;
[0007] (2) Kneading: The mixed material is placed at 120-130°C for drying for 20-24 hours, then kneaded for 5-10 minutes, heated to 165-170°C, and then the modified filler is added, and kneaded for another 10-15 minutes to obtain a modified material;
[0008] (3) Molding: placing the modified material in a mold and vibrating the mold to obtain a green body;
[0009] (4) Calcination: The green body is placed in a calcination furnace and calcined at a gradient temperature to obtain a pre-baked anode with a high volume density;
[0010] Furthermore, the preparation method of the modifier is as follows:
[0011] S1: Disperse graphene quantum dots in a mixture of ethanol and deionized water, then add triethoxyvinylsilane, stir in an ice water bath for 30-40 minutes, then heat to 60-70°C, stir for 1-2 hours, wash, and dry to obtain olefinic quantum dots.
[0012] S2: adding sulfur to dimethyl sulfoxide, heating at 160-165° C. for 30-40 min, then adding olefinic quantum dots and methoxy-polyethylene glycol-thiol, stirring for 9-10 h, filtering, washing, and drying to obtain a modified filler;
[0013] Preferably, in step S1, the weight ratio of graphene quantum dots, ethanol, deionized water and triethoxyvinylsilane is 5-10:10-20:50-100:0.5-2;
[0014] Preferably, in step S2, the weight ratio of sulfur, dimethyl sulfoxide, olefinic quantum dots and methoxy-polyethylene glycol-thiol is 1-2:50-100:5-10:0.1-0.5.
[0015] Preferably, the preparation method of calcined coke in step (1) is as follows: the calcined petroleum coke raw material is ground and screened, and the weight percentage of each particle size material in the calcined coke after screening is: the content of particle size 6-8mm is 14wt%, the content of particle size 3-6mm is 20wt%, the content of particle size 0.05-3mm is 40wt%, and the content of particle size less than 0.05mm is 26wt%.
[0016] Preferably, the coal tar pitch in step (1) is modified asphalt.
[0017] Preferably, the softening point of the modified asphalt is 100-115°C, the toluene insoluble content is 30-34wt%, the quinoline insoluble content is 8-10wt%, the β-resin content is 20-25wt%, the coking value is 55-58wt%, and the ash content is less than 0.3wt%.
[0018] Preferably, in step (1), the weight ratio of calcined coke to coal tar pitch is 4:1.
[0019] Preferably, the weight ratio of the mixed material to the modified filler in step (2) is 10:0.5-1.
[0020] Preferably, the exciting force of the vibration molding in step (3) is 300-400 KN, the molding temperature is 160-170° C., and the vibration time is 120-140 s.
[0021] Preferably, the step of gradient temperature rise roasting in step (4) is: heating the roasting furnace to 650°C at a heating rate of 5°C / h, preheating for 2-3h, then heating to 1250°C at a heating rate of 15°C / h, keeping warm for 80-90h, and removing from the furnace after cooling.
[0022] Preferably, the weight average molecular weight of the methoxy-polyethylene glycol-thiol in step S2 is 500.
[0023] Furthermore, the present invention also provides a prebaked anode with high volume density, which is obtained by the above-mentioned method for preparing the prebaked anode with high volume density.
[0024] Furthermore, the present invention also provides an application of a high volume density prebaked anode in aluminum electrolysis.
[0025] Beneficial effects of the present invention:
[0026] The present invention provides a prebaked anode with high volume density, wherein a modified filler is added during the kneading process so that the volume density can reach 1.95 g·cm -3 Moreover, it has lower porosity, resistivity and higher compressive strength, which has great practical significance for aluminum electrolysis production.
[0027] The modified filler provided by the present invention is obtained by simultaneously grafting sulfur polymer and polyether onto graphene quantum dots modified by alkenyl silane coupling agent. The sulfur polymer and polyether can synergistically change the surface properties of the graphene quantum dots so that the graphene quantum dots are effectively dispersed in the prebaked anode. The sulfur polymer can further sulfurize the coal tar pitch and enhance the interaction between the graphene quantum dots and the coal tar pitch, thereby increasing the volume density of the prebaked anode and reducing the porosity and resistivity. In addition, due to the reinforcing effect of the graphene quantum dots, the compressive strength of the prebaked anode is as high as 64MPa. DETAILED DESCRIPTION
[0028] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.
[0029] The flake diameter of the graphene quantum dots in the specific implementation manner of the present invention is 3-6nm; the weight average molecular weight of methoxy-polyethylene glycol-thiol is 500; the weight percentage of each particle size material in the calcined coke is: the content of particle size 6-8mm is 14wt%, the content of particle size 3-6mm is 20wt%, the content of particle size 0.05-3mm is 40wt%, and the content of particle size below 0.05mm is 26wt%; the softening point of the modified asphalt is 108°C, the content of toluene insoluble matter is 32wt%, the content of quinoline insoluble matter is 8.5wt%, the content of β-resin is 22wt%, the coking value is 56wt%, and the ash content is 0.2wt%.
[0030] Preparation Example 1:
[0031] S1: Disperse 5 g of graphene quantum dots in a mixture of 10 g of ethanol and 50 g of deionized water, then add 0.5 g of triethoxyvinylsilane, stir in an ice-water bath for 30 min, then heat to 60°C, stir and react for 1 h, wash, and dry to obtain olefinic quantum dots.
[0032] S2: Add 1 g of sulfur to 50 g of dimethyl sulfoxide, heat at 160°C for 30 min, then add 5 g of olefinated quantum dots and 0.1 g of methoxy-polyethylene glycol-thiol, stir for 9 h, filter, wash, and dry to obtain a modified filler.
[0033] Preparation Example 2:
[0034] S1: Disperse 7.5 g of graphene quantum dots in a mixture of 15 g of ethanol and 85 g of deionized water, then add 1 g of triethoxyvinylsilane, stir in an ice-water bath for 35 min, then heat to 65°C, stir and react for 1.5 h, wash, and dry to obtain olefinic quantum dots.
[0035] S2: Add 1.5 g of sulfur to 80 g of dimethyl sulfoxide, heat at 160° C. for 40 min, then add 7.5 g of olefinic quantum dots and 0.3 g of methoxy-polyethylene glycol-thiol, stir for 10 h, filter, wash, and dry to obtain a modified filler.
[0036] Preparation Example 3:
[0037] S1: Disperse 10 g of graphene quantum dots in a mixture of 20 g of ethanol and 100 g of deionized water, then add 2 g of triethoxyvinylsilane, stir in an ice-water bath for 40 min, then heat to 70°C, stir and react for 2 h, wash, and dry to obtain olefinic quantum dots.
[0038] S2: Add 2 g of sulfur to 100 g of dimethyl sulfoxide, heat at 165° C. for 40 min, then add 10 g of olefinic quantum dots and 0.5 g of methoxy-polyethylene glycol-thiol, stir for 10 h, filter, wash, and dry to obtain a modified filler.
[0039] Preparation Example 4:
[0040] S1: Add 1.5 g of sulfur to 80 g of dimethyl sulfoxide, heat at 160° C. for 40 min, then add 7.5 g of graphene quantum dots and 0.3 g of methoxy-polyethylene glycol-thiol, stir for 10 h, filter, wash, and dry to obtain a modified filler.
[0041] Preparation Example 5:
[0042] S1: Disperse 7.5 g of graphene quantum dots in a mixture of 15 g of ethanol and 85 g of deionized water, then add 1 g of triethoxyvinylsilane, stir in an ice-water bath for 35 min, then heat to 65°C, stir and react for 1.5 h, wash, and dry to obtain olefinic quantum dots.
[0043] S2: 1.5 g of sulfur was added to 80 g of dimethyl sulfoxide, heated at 160° C. for 40 min, and then 7.5 g of olefinic quantum dots were added, stirred for 10 h, filtered, washed, and dried to obtain a modified filler.
[0044] Embodiment 1:
[0045] (1) Mixing: 40 g of calcined coke and 10 g of modified asphalt were mixed to form a mixed material;
[0046] (2) Kneading: 50 g of the mixed material was dried at 120° C. for 20 h, then kneaded for 5 min, heated to 165° C., and then 2.5 g of the modified filler prepared in Preparation Example 1 was added, and kneaded for another 10 min to obtain a modified material;
[0047] (3) Molding: The modified material is placed in a mold and vibrated to obtain a green body; the excitation force of the vibration molding is 300 KN, the molding temperature is 160° C., and the vibration time is 120 s;
[0048] (4) Calcination: Place the green body in a calcination furnace, heat the calcination furnace to 650°C at a heating rate of 5°C / h, preheat for 2h, then heat to 1250°C at a heating rate of 15°C / h, keep warm for 80h, cool and take out to obtain a prebaked anode with high volume density.
[0049] Embodiment 2:
[0050] (1) Mixing: 40 g of calcined coke and 10 g of modified asphalt were mixed to form a mixed material;
[0051] (2) Kneading: 50 g of the mixed material was dried at 125° C. for 22 h, then kneaded for 8 min, heated to 170° C., and then 4 g of the modified filler prepared in Preparation Example 2 was added, and kneaded for another 12 min to obtain a modified material;
[0052] (3) Molding: placing the modified material in a mold and vibrating the mold. The excitation force of the vibration molding is 350 KN, the molding temperature is 165 ° C, and the vibration time is 130 s to obtain a green body;
[0053] (4) Calcination: Place the green body in a calcination furnace, heat the calcination furnace to 650°C at a heating rate of 5°C / h, preheat for 2.5 hours, then heat to 1250°C at a heating rate of 15°C / h, keep warm for 85 hours, and then cool and take out to obtain a prebaked anode with high volume density.
[0054] Embodiment 3:
[0055] (1) Mixing: 40 g of calcined coke and 10 g of modified asphalt were mixed to form a mixed material;
[0056] (2) Kneading: 50 g of the mixed material was placed at 130° C. and dried for 24 h, then kneaded for 10 min, heated to 170° C., and then 5 g of the modified filler prepared in Preparation Example 3 was added, and kneaded for another 15 min to obtain a modified material;
[0057] (3) Molding: The modified material is placed in a mold and vibrated to obtain a green body; the excitation force of the vibration molding is 400 KN, the molding temperature is 170° C., and the vibration time is 140 s;
[0058] (4) Calcination: Place the green body in a calcination furnace, heat the calcination furnace to 650°C at a heating rate of 5°C / h, preheat for 3 hours, then heat to 1250°C at a heating rate of 15°C / h, keep warm for 90 hours, cool and take out to obtain a prebaked anode with high volume density.
[0059] Comparative Example 1:
[0060] (1) Mixing: 40 g of calcined coke and 10 g of modified asphalt were mixed to form a mixed material;
[0061] (2) Kneading: 50 g of the mixed material was placed at 125 °C for 22 h, then kneaded for 8 min, heated to 170 °C, and then 4 g of graphene quantum dots were added, and kneaded for another 12 min to obtain a modified material;
[0062] (3) Molding: placing the modified material in a mold and vibrating the mold. The excitation force of the vibration molding is 350 KN, the molding temperature is 165 ° C, and the vibration time is 130 s to obtain a green body;
[0063] (4) Calcination: Place the green body in a calcination furnace, heat the calcination furnace to 650°C at a heating rate of 5°C / h, preheat for 2.5h, then heat to 1250°C at a heating rate of 15°C / h, keep warm for 85h, cool and take out to obtain a prebaked anode.
[0064] Comparative Example 2:
[0065] (1) Mixing: 40 g of calcined coke and 10 g of modified asphalt were mixed to form a mixed material;
[0066] (2) Kneading: 50 g of the mixed material was dried at 125° C. for 22 h, then kneaded for 8 min, heated to 170° C., and then 4 g of the modified filler prepared in Preparation Example 4 was added, and kneaded for another 12 min to obtain a modified material;
[0067] (3) Molding: placing the modified material in a mold and vibrating the mold. The excitation force of the vibration molding is 350 KN, the molding temperature is 165 ° C, and the vibration time is 130 s to obtain a green body;
[0068] (4) Calcination: Place the green body in a calcination furnace, heat the calcination furnace to 650°C at a heating rate of 5°C / h, preheat for 2.5h, then heat to 1250°C at a heating rate of 15°C / h, keep warm for 85h, cool and take out to obtain a prebaked anode.
[0069] Comparative Example 3:
[0070] (1) Mixing: 40 g of calcined coke and 10 g of modified asphalt were mixed to form a mixed material;
[0071] (2) Kneading: 50 g of the mixed material was dried at 125° C. for 22 h, then kneaded for 8 min, heated to 170° C., and then 4 g of the modified filler prepared in Preparation Example 5 was added, and kneaded for another 12 min to obtain a modified material;
[0072] (3) Molding: placing the modified material in a mold and vibrating the mold. The excitation force of the vibration molding is 350 KN, the molding temperature is 165 ° C, and the vibration time is 130 s to obtain a green body;
[0073] (4) Calcination: Place the green body in a calcination furnace, heat the calcination furnace to 650°C at a heating rate of 5°C / h, preheat for 2.5h, then heat to 1250°C at a heating rate of 15°C / h, keep warm for 85h, cool and take out to obtain a prebaked anode.
[0074] Comparative Example 4:
[0075] (1) Mixing: 40 g of calcined coke and 10 g of modified asphalt were mixed to form a mixed material;
[0076] (2) Kneading: 50 g of the mixed material was dried at 125°C for 22 h, then kneaded for 8 min, heated to 170°C, and kneaded for another 12 min to obtain a modified material;
[0077] (3) Molding: placing the modified material in a mold and vibrating the mold. The excitation force of the vibration molding is 350 KN, the molding temperature is 165 ° C, and the vibration time is 130 s to obtain a green body;
[0078] (4) Calcination: Place the green body in a calcination furnace, heat the calcination furnace to 650°C at a heating rate of 5°C / h, preheat for 2.5h, then heat to 1250°C at a heating rate of 15°C / h, keep warm for 85h, cool and take out to obtain a prebaked anode.
[0079] Performance Testing:
[0080] Bulk density: measured according to GB / T6154-1985; porosity: measured according to YB / T 908-1978; compressive strength: measured by a universal testing machine; resistivity: measured by a resistivity tester; reactivity: air reactivity is measured by an air reactivity tester, and CO2 reactivity is measured by a CO2 reactivity tester. The results are shown in Table 1.
[0081] Table 1 Performance test data
[0082]
[0083]
[0084] Data Analysis:
[0085] It can be seen from the performance test data of Examples 1-3 that the high volume density prebaked anode prepared by the present invention has a high volume density, which can reach 1.95 g·cm -3 , and has a lower porosity. The high volume density and low porosity indicate that the modified filler effectively fills the pores formed by the thermal decomposition and condensation of coal tar during the roasting process, and has a certain reinforcing effect, so that the compressive strength can reach more than 61MPa. It is worth mentioning that the modified filler can further reduce the resistivity.
[0086] It can be seen from the performance test data of Example 2 and Comparative Examples 1-4 that the surface modification of graphene quantum dots is crucial to improving the performance of prebaked anodes, especially the improvement of volume density. Directly adding graphene quantum dots to the raw materials of prebaked anodes can improve the volume density. This is mainly due to the filling effect of graphene quantum dots. After the graphene quantum dots are olefinated, polyethers and sulfur polymers can be grafted on their surfaces at the same time. The polyethers and sulfur polymers change the surface properties of graphene quantum dots, thereby making them more effectively play a filling role. In addition, the sulfur polymer itself can sulfurize the modified asphalt, thereby building a strong interaction between the modified asphalt and the graphene quantum dots, thereby further improving the volume density.
[0087] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.
Claims
1. A method for preparing a prebaked anode with high volume density, characterized in that: The following steps are involved: (1) Mixing: mixing calcined coke and coal tar pitch; (2) Kneading: The mixed material is placed at 120-130°C for drying for 20-24 hours, then kneaded for 5-10 minutes, heated to 165-170°C, and then the modified filler is added, and kneaded for another 10-15 minutes to obtain a modified material; (3) Molding: placing the modified material in a mold and vibrating the mold to obtain a green body; (4) Calcination: The green body is placed in a calcination furnace and calcined at a gradient temperature to obtain a pre-baked anode with a high volume density; The preparation method of the modifier is as follows: S1: Disperse graphene quantum dots in a mixture of ethanol and deionized water, then add triethoxyvinylsilane, stir in an ice water bath for 30-40 minutes, then heat to 60-70°C, stir for 1-2 hours, wash, and dry to obtain olefinic quantum dots. S2: adding sulfur to dimethyl sulfoxide, heating at 160-165° C. for 30-40 min, then adding olefinic quantum dots and methoxy-polyethylene glycol-thiol, stirring for 9-10 h, filtering, washing, and drying to obtain a modified filler; In the step S1, the weight ratio of graphene quantum dots, ethanol, deionized water and triethoxyvinylsilane is 5-10:10-20:50-100:0.5-2; In the step S2, the weight ratio of sulfur, dimethyl sulfoxide, olefinic quantum dots and methoxy-polyethylene glycol-thiol is 1-2:50-100:5-10:0.1-0.
5.
2. The method for preparing a prebaked anode with a high volume density according to claim 1, wherein the method for preparing the calcined coke in step (1) is as follows: the calcined petroleum coke raw material is ground and screened, and the weight percentage of each particle size material in the calcined coke after screening is: the content of the particle size of 6-8mm is 14wt%, the content of the particle size of 3-6mm is 20wt%, the content of the particle size of 0.05-3mm is 40wt%, and the content of the particle size below 0.05mm is 26wt%.
3. According to the method for preparing a prebaked anode with high volume density as claimed in claim 1, the coal tar pitch in step (1) is modified asphalt.
4. The method for preparing a prebaked anode with high volume density according to claim 3, characterized in that: The modified asphalt has a softening point of 100-115° C., a toluene insoluble content of 30-34wt%, a quinoline insoluble content of 8-10wt%, a β-resin content of 20-25wt%, a coking value of 55-58wt%, and an ash content of less than 0.3wt%.
5. The method for preparing a prebaked anode with high volume density according to claim 1, characterized in that: In the step (1), the weight ratio of calcined coke to coal tar pitch is 4:
1.
6. The method for preparing a prebaked anode with high volume density according to claim 1, characterized in that: The weight ratio of the mixed material to the modified filler in the step (2) is 10:0.5-1.
7. The method for preparing a prebaked anode with a high volume density according to claim 1, characterized in that: In the step (3), the exciting force of the vibration molding is 300-400 KN, the molding temperature is 160-170° C., and the vibration time is 120-140 s.
8. The method for preparing a prebaked anode with high volume density according to claim 1, characterized in that: The step of gradient temperature rise roasting in step (4) is as follows: heat the roasting furnace to 650°C at a heating rate of 5°C / h, preheat for 2-3h, then heat to 1250°C at a heating rate of 15°C / h, keep warm for 80-90h, and remove from the furnace after cooling.
9. The method for preparing a prebaked anode with high volume density according to claim 1, characterized in that: The weight average molecular weight of the methoxy-polyethylene glycol-thiol in step S2 is 500.
10. An application of a prebaked anode with high volume density obtained by the method for preparing a prebaked anode with high volume density according to any one of claims 1 to 9, characterized in that: Used for aluminum electrolysis.
Citation Information
Patent Citations
Vinyl silane modified graphene oxide composite material as well as preparation method and application thereof
CN113185858A
Preparation method of efficient prebaked anode for aluminum electrolysis starting tank
CN114773064A
Photovoltaic isostatic pressing graphite as well as preparation method and application thereof
CN116462509A
Method and device for preparing graphene-based polyethylene glycol phase change material
US11339316B1
Method of manufacturing multi-structural high-heat-dissipation part having controlled packing density of carbon material, and multi-structural high-heat-dissipation part manufactured thereby
US20200196435A1
Cited By
Aluminum electrolysis anode scrap sealing paste based on special phenolic resin and preparation method of aluminum electrolysis anode scrap sealing paste
CN121342531A