Coal gangue brick fully utilizing waste resources and preparation method thereof

Through the preparation process of treating coal gangue bricks with graphene oxide treatment liquid and reinforcement treatment agent, the problem of low strength of existing permeable bricks is solved, and coal gangue bricks with high compressive strength and permeability are achieved, making full use of waste resources. Improve the environmental protection performance of building materials.

CN119039034AInactive Publication Date: 2024-11-29JIAHE COUNTY BAOHU BUILDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411143770.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent
Patent Text Reader

Abstract

The invention discloses a coal gangue brick fully utilizing waste resources and a preparation method thereof, and belongs to the technical field of building materials.The preparation method comprises the steps that a mixture is subjected to compression molding and drying in a mold, then the mixture is transferred into a sintering furnace to be subjected to heat preservation for 60-90 min at the temperature of 550-600 DEG C, natural cooling is conducted, a pre-sintered brick blank is obtained, the pre-sintered brick blank is soaked with a reinforcing treating agent till the water content is 10-15%, drying is conducted, and the coal gangue brick is obtained. And then transferring the mixture into a sintering furnace for heat preservation for 45-60 minutes at 250-300 DEG C, for heat preservation for 60-90 minutes at 900-950 DEG C and for heat preservation for 60-90 minutes at 1200-1250 DEG C, and naturally cooling to obtain the coal gangue brick fully utilizing waste resources. Coal gangue waste resources and concrete waste resources are fully utilized, and after the coal gangue waste resources and the concrete waste resources are blended, the prepared coal gangue brick has high compressive strength and water permeability coefficient and is conveniently applied to urban roads.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and particularly relates to a gangue brick which fully utilizes waste resources and a preparation method thereof. Background Art

[0002] As an important part of the construction industry, the research on brickwork construction technology has become more mature. Only by improving the scientificity and rationality of brickwork construction technology can the quality of house construction be guaranteed. In the past, solid bricks sintered with clay were generally used. Solid bricks not only have low strength and seismic resistance, poor heat insulation and sound insulation, but also occupy a large amount of land resources and cause environmental damage.

[0003] Gangue bricks are building materials made from gangue or slag discharged from coal mines as the main raw materials. They have the advantages of environmental protection, light weight, high strength, thermal insulation and fire resistance. They not only save land and energy, but also realize the recycling of waste. In order to expand the utilization of waste resources, there are related applications of preparing permeable bricks with gangue mixed with construction waste. Construction waste includes bricks, tiles, concrete blocks, glass, sand and gravel, and waste wood, etc., with complex components. Modern construction waste is mainly concrete. When permeable bricks are fired as raw materials, the CSH gel network structure in it is destroyed at high temperatures. In addition, there is a difference in the thermal expansion coefficients of waste concrete and gangue, which leads to cracks and reduces the strength of permeable bricks. Therefore, when preparing permeable bricks, the amount of waste concrete is generally not high, which is not conducive to the full utilization of waste concrete resources. Summary of the invention

[0004] The purpose of the present invention is to provide a coal gangue brick which fully utilizes waste resources and a preparation method thereof, and to improve the strength of the coal gangue brick mixed with high-content concrete waste resources by treating with the prepared reinforcing treatment agent.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] A method for preparing coal gangue bricks by fully utilizing waste resources comprises the following steps:

[0007] Step 1: crush the waste concrete into particles with a particle size of 5-10 mm, evenly spray the graphene oxide treatment liquid on the surface of the particles at a ratio of 10 kg: 1 L, and obtain pretreated concrete aggregate after natural drying;

[0008] Step 2: crushing the gangue, screening out the gangue coarse aggregate with a particle size of 5-10 mm and the gangue fine aggregate with a particle size of 2-4 mm; crushing the sieved gangue to a particle size of less than 0.45 mm to obtain gangue sand; mixing the gangue coarse aggregate, the gangue fine aggregate, the gangue sand and the pre-treated concrete aggregate, then adding clean water and stirring evenly, then adding kaolin with a particle size of less than 0.2 mm and potassium feldspar with a particle size of less than 0.2 mm, stirring evenly to obtain a mixture;

[0009] Step 3: Press the mixture into a mold with a pressure of 22-25kg / cm 2 , drying the obtained bricks at 60-80°C, then transferring them to a sintering furnace, heating them to 550-600°C at a rate of 3-5°C / min, keeping them at that temperature for 60-90min, and cooling them naturally to obtain pre-sintered bricks;

[0010] Step 4: Soak the pre-sintered brick blank with a reinforcing treatment agent to a moisture content of 10-15%, dry at 60-80°C, then transfer it to a sintering furnace, heat it to 250-300°C at a rate of 3-5°C / min, keep it warm for 45-60min, then heat it to 900-950°C at a rate of 5-10°C / min, keep it warm for 60-90min, then heat it to 1200-1250°C at a rate of 5-10°C / min, keep it warm for 60-90min, cool it naturally to obtain coal gangue bricks, and complete the preparation method of coal gangue bricks that fully utilize waste resources.

[0011] Furthermore, the mass ratio of the gangue coarse aggregate, the gangue fine aggregate, the gangue sand, the pre-treated concrete aggregate, the clean water, the kaolin and the potassium feldspar is 5-10:15-25:45-60:80-120:9-14:6-12:12-18.

[0012] Further, the graphene oxide treatment solution is prepared by the following steps:

[0013] Graphite and sodium nitrate are added to a reactor, concentrated sulfuric acid with a mass fraction of 98% is added to the reactor at 0-5°C and stirred for 1.5-2h to allow the concentrated sulfuric acid to be fully inserted into the graphite layers, potassium permanganate is added to the reactor and stirring is continued for 7-8h, hot water at 70°C is passed into the reactor and stirring is continued for 1.5-2h, and then a hydrogen peroxide solution with a mass fraction of 30% is added, stirring is continued for 1h to remove the potassium permanganate, the precipitate is allowed to stand to obtain the precipitate, the precipitate is washed with deionized water until the last washing liquid is neutral, and dried to obtain graphene oxide.

[0014] Graphene oxide, hydroxypropyl cellulose and deionized water were added into a reactor at a mass ratio of 1:1:1000, stirred and mixed, and ultrasonically dispersed for 20-30 minutes to obtain a graphene oxide treatment solution.

[0015] Furthermore, the usage ratio of graphite, sodium nitrate, concentrated sulfuric acid, potassium permanganate, hot water and hydrogen peroxide is 2-4g:1-2g:200-400mL:8-15g:200-400mL:80-100mL.

[0016] Furthermore, the reinforcing treatment agent is prepared by the following steps:

[0017] Step 1: Add deionized water, formic acid and acetic acid into a reactor, stir at 200-300 r / min for 5-10 min, heat to 85-90° C., add aluminum powder into the reactor, continue stirring for 2.5-3 h, add nitric acid with a mass fraction of 68% into the reactor, keep warm for 18-20 h, and obtain aluminum carboxylate sol;

[0018] Furthermore, the mass ratio of deionized water, formic acid, acetic acid, aluminum powder and nitric acid is 500:30:36:27:32.

[0019] Step 2: adding tetramethyltetravinylcyclotetrasiloxane and polymethylhydrogensiloxane into a reaction kettle, stirring for 20-30 minutes at 20-25° C. and 200-300 r / min, then adding nano magnesium oxide powder and nano zirconium oxide powder into the reaction kettle, and continuing to stir for 20-30 minutes to obtain a nanoparticle dispersion;

[0020] Furthermore, the usage ratio of tetramethyltetravinylcyclotetrasiloxane, polymethylhydrogensiloxane, nano magnesium oxide powder and nano zirconium oxide powder is 68-70:44-45:5-6:5-6.

[0021] Step 3: Stir and mix the aluminum carboxylate sol and the nanoparticle dispersion in a mass ratio of 5:1 to obtain a reinforcing treatment agent.

[0022] Beneficial effects of the present invention:

[0023] The gangue brick of the present invention is prepared by a sintering method, which makes full use of waste gangue resources and waste concrete resources. After the gangue brick is mixed with waste gangue resources and waste concrete resources, the prepared gangue brick has high compressive strength and water permeability coefficient, and is convenient for application in urban roads.

[0024] In the preparation process of the coal gangue brick of the present invention, the waste concrete aggregate is first treated with a graphene oxide treatment liquid. Hydroxypropyl cellulose helps to improve the dispersibility and adhesion of graphene oxide. Graphene oxide can promote the mutual cross-linking between microcrystals of the pretreated concrete aggregate, improve the heat resistance and strength of the pretreated concrete aggregate, reduce the generation of cracks during the firing process, and help to ensure the compressive strength of the coal gangue brick under a high waste concrete content.

[0025] The brick blank of the present invention is first pre-sintered to avoid rapid evaporation of water and volatile components in the brick blank, which helps to reduce cracking or deformation and ensure the porosity inside the pre-sintered brick blank; the reinforcing treatment agent is obtained by mixing carboxylic acid aluminum sol and nanoparticle dispersion liquid, and the liquid phase of the nanoparticle dispersion liquid includes tetramethyltetravinylcyclotetrasiloxane and polymethylhydrogensiloxane with good stability, which helps nano magnesium oxide and nano zirconium oxide to be evenly dispersed in the carboxylic acid aluminum sol and prevents the nano particles from agglomerating; after the pre-sintered brick blank is soaked with the reinforcing treatment agent, the reinforcing treatment agent is attached to the pore network of the pre-sintered brick blank, and the reinforcing treatment agent is promoted to form a tetramethyl tetravinylcyclotetrasiloxane under a temperature of 250-300°C. The carbon-carbon double bonds in methyltetravinylcyclotetrasiloxane and the silicon-hydrogen bonds in polymethylhydrogensiloxane are cross-linked and solidified, further improving the structural stability of the pre-sintered brick. Under the temperature of 900-950℃, the organic siloxane is pyrolyzed to form amorphous ceramics such as silicon carbide, and aluminum carboxylate is converted into aluminum oxide. The gas produced by the decomposition of organic matter has the function of forming holes and passing holes. Nano-magnesium oxide and nano-zirconium oxide play a role of solid solution. Finally, the brick is fired and formed at 1200-1250℃ to form a denser ceramic material at the bonding position, retaining the effective pores inside the gangue brick, ensuring water permeability while improving the compressive strength of the gangue brick. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Example 1: This example provides a coal gangue brick that fully utilizes waste resources, which is prepared by the following method:

[0028] S1: 20 kg of graphite and 10 kg of sodium nitrate are added to a reactor, 2000 L of 98% concentrated sulfuric acid is added to the reactor at 0°C and stirred for 1.5 h to allow the concentrated sulfuric acid to fully insert into the graphite layers, 80 kg of potassium permanganate is added to the reactor and stirring is continued for 7 h, 2000 L of 70°C hot water is passed into the reactor and stirring is continued for 1.5 h, then 800 L of 30% hydrogen peroxide solution is added and stirring is continued for 1 h to remove the potassium permanganate, the mixture is allowed to stand to obtain a precipitate, the precipitate is washed with deionized water until the last washing liquid is neutral, and dried to obtain graphene oxide; graphene oxide, hydroxypropyl cellulose and deionized water are added to the reactor in a mass ratio of 1:1:1000, stirred and mixed, and ultrasonically dispersed for 20 min to obtain a graphene oxide treatment solution for standby use.

[0029] S2: Add 5000kg of deionized water, 30kg of formic acid and 36kg of acetic acid into a reactor, stir at 200r / min for 5min, heat to 85°C, add 27kg of aluminum powder into the reactor, continue stirring for 2.5h, add 32kg of nitric acid with a mass fraction of 68% into the reactor, keep warm and react for 18h to obtain carboxylate aluminum sol; add 680kg of tetramethyltetravinylcyclotetrasiloxane and 440kg of polymethylhydrogensiloxane into the reactor, stir at 20°C and 200r / min for 20min, then add 5kg of nano magnesium oxide powder and 5kg of nano zirconium oxide powder into the reactor, continue stirring for 20min to obtain a nanoparticle dispersion; stir and mix the carboxylate aluminum sol and the nanoparticle dispersion in a mass ratio of 5:1 to obtain a reinforcing treatment agent for standby use.

[0030] S3: crush the waste concrete into particles with a particle size of 5-10 mm, spray the graphene oxide treatment liquid evenly on the surface of the particles at a ratio of 10 kg: 1 L, and obtain pretreated concrete aggregate after natural drying.

[0031] S4: crushing the gangue, screening out the gangue coarse aggregate with a particle size of 5-10 mm and the gangue fine aggregate with a particle size of 2-4 mm; crushing the screened gangue to a particle size of less than 0.45 mm to obtain gangue sand; mixing 5 kg of the gangue coarse aggregate, 15 kg of the gangue fine aggregate, 45 kg of the gangue sand and 80 kg of the pretreated concrete aggregate, then adding 9 kg of clean water and stirring evenly, then adding 6 kg of kaolin with a particle size of less than 0.2 mm and 12 kg of potassium feldspar with a particle size of less than 0.2 mm, stirring evenly to obtain a mixture.

[0032] S5: Press the mixture into a mold at a pressure of 22 kg / cm 2 The obtained bricks were dried at 60°C, then transferred to a sintering furnace, heated to 550°C at a rate of 3°C / min, kept warm for 60 minutes, and naturally cooled to obtain pre-sintered bricks.

[0033] S6: Soak the pre-sintered brick blank with a reinforcing treatment agent to a moisture content of 10%, dry at 60°C, then transfer to a sintering furnace, heat to 250°C at a rate of 3°C / min, keep warm for 45 minutes, then heat to 900°C at a rate of 5°C / min, keep warm for 60 minutes, then heat to 1200°C at a rate of 5°C / min, keep warm for 60 minutes, cool naturally to obtain gangue bricks, and complete the preparation method of gangue bricks that fully utilize waste resources.

[0034] Example 2: This example provides a coal gangue brick that fully utilizes waste resources, which is prepared by the following method:

[0035] S1: 30 kg of graphite and 15 kg of sodium nitrate are added to a reactor, 3000 L of 98% concentrated sulfuric acid is added to the reactor at 2°C and stirred for 1.8 h to allow the concentrated sulfuric acid to fully insert into the graphite layers, 115 kg of potassium permanganate is added to the reactor and stirring is continued for 7.5 h, 3000 L of 70°C hot water is passed into the reactor and stirring is continued for 1.8 h, and then 900 L of 30% hydrogen peroxide solution is added, stirring is continued for 1 h to remove potassium permanganate, the precipitate is allowed to stand and washed with deionized water until the last washing liquid is neutral, and dried to obtain graphene oxide; graphene oxide, hydroxypropyl cellulose and deionized water are added to the reactor in a mass ratio of 1:1:1000, stirred and mixed, and ultrasonically dispersed for 25 min to obtain a graphene oxide treatment solution for standby use.

[0036] S2: Add 5000kg of deionized water, 30kg of formic acid and 36kg of acetic acid into a reactor, stir at 250r / min for 8min, heat to 88°C, add 27kg of aluminum powder into the reactor, continue stirring for 2.8h, add 32kg of nitric acid with a mass fraction of 68% into the reactor, keep warm and react for 19h to obtain carboxylate aluminum sol; add 690kg of tetramethyltetravinylcyclotetrasiloxane and 445kg of polymethylhydrogensiloxane into the reactor, stir at 22°C and 250r / min for 25min, then add 5.5kg of nano magnesium oxide powder and 5.5kg of nano zirconium oxide powder into the reactor, continue stirring for 25min to obtain a nanoparticle dispersion; stir and mix the carboxylate aluminum sol and the nanoparticle dispersion in a mass ratio of 5:1 to obtain a reinforcing treatment agent for standby use.

[0037] S3: crush the waste concrete into particles with a particle size of 5-10 mm, spray the graphene oxide treatment liquid evenly on the surface of the particles at a ratio of 10 kg: 1 L, and obtain pretreated concrete aggregate after natural drying.

[0038] S4: crushing the gangue, screening out the gangue coarse aggregate with a particle size of 5-10 mm and the gangue fine aggregate with a particle size of 2-4 mm; crushing the screened gangue to a particle size of less than 0.45 mm to obtain gangue sand; mixing 7.5 kg of the gangue coarse aggregate, 20 kg of the gangue fine aggregate, 52.5 kg of the gangue sand and 100 kg of the pretreated concrete aggregate, then adding 11.5 kg of clean water and stirring evenly, then adding 9 kg of kaolin with a particle size of less than 0.2 mm and 15 kg of potassium feldspar with a particle size of less than 0.2 mm, stirring evenly to obtain a mixture.

[0039] S5: The mixture is pressed into a mold at a pressure of 23.5 kg / cm 2The obtained bricks were dried at 70°C, then transferred to a sintering furnace, heated to 580°C at a rate of 4°C / min, kept warm for 75 minutes, and naturally cooled to obtain pre-sintered bricks.

[0040] S6: Soak the pre-fired bricks with a reinforcing treatment agent until the moisture content is 12.5%, dry at 70°C, then transfer to a sintering furnace, heat to 280°C at a rate of 4°C / min, keep warm for 50 minutes, then heat to 925°C at a rate of 8°C / min, keep warm for 75 minutes, then heat to 1230°C at a rate of 8°C / min, keep warm for 75 minutes, cool naturally to obtain gangue bricks, and complete the preparation method of gangue bricks that fully utilize waste resources.

[0041] Example 3: This example provides a coal gangue brick that fully utilizes waste resources, which is prepared by the following method:

[0042] S1: 40 kg of graphite and 20 kg of sodium nitrate are added to a reactor, 4000 L of 98% concentrated sulfuric acid is added to the reactor at 5°C and stirred for 2 h to allow the concentrated sulfuric acid to fully insert into the graphite layers, 150 kg of potassium permanganate is added to the reactor and stirring is continued for 8 h, 4000 L of 70°C hot water is passed into the reactor and stirring is continued for 2 h, then 1000 L of 30% hydrogen peroxide solution is added and stirring is continued for 1 h to remove the potassium permanganate, the solution is allowed to stand to obtain a precipitate, the precipitate is washed with deionized water until the last washing solution is neutral, and dried to obtain graphene oxide; graphene oxide, hydroxypropyl cellulose and deionized water are added to the reactor in a mass ratio of 1:1:1000, stirred and mixed, and ultrasonically dispersed for 30 min to obtain a graphene oxide treatment solution for standby use.

[0043] S2: Add 5000kg of deionized water, 30kg of formic acid and 36kg of acetic acid into a reactor, stir at 300r / min for 10min, heat to 90°C and add 27kg of aluminum powder into the reactor, continue stirring for 3h, add 32kg of nitric acid with a mass fraction of 68% into the reactor, keep warm and react for 20h to obtain carboxylate aluminum sol; add 700kg of tetramethyltetravinylcyclotetrasiloxane and 450kg of polymethylhydrogensiloxane into the reactor, stir at 25°C and 300r / min for 30min, then add 6kg of nano magnesium oxide powder and 6kg of nano zirconium oxide powder into the reactor, continue stirring for 30min to obtain a nanoparticle dispersion; stir and mix the carboxylate aluminum sol and the nanoparticle dispersion in a mass ratio of 5:1 to obtain a reinforcing treatment agent for standby use.

[0044] S3: crush the waste concrete into particles with a particle size of 5-10 mm, spray the graphene oxide treatment liquid evenly on the surface of the particles at a ratio of 10 kg: 1 L, and obtain pretreated concrete aggregate after natural drying.

[0045] S4: crushing the gangue, screening out the gangue coarse aggregate with a particle size of 5-10 mm and the gangue fine aggregate with a particle size of 2-4 mm; crushing the screened gangue to a particle size of less than 0.45 mm to obtain gangue sand; mixing 10 kg of the gangue coarse aggregate, 25 kg of the gangue fine aggregate, 60 kg of the gangue sand and 120 kg of the pretreated concrete aggregate, then adding 14 kg of clean water and stirring evenly, then adding 12 kg of kaolin with a particle size of less than 0.2 mm and 18 kg of potassium feldspar with a particle size of less than 0.2 mm, stirring evenly to obtain a mixture.

[0046] S5: Press the mixture into a mold at a pressure of 25 kg / cm 2 The obtained bricks were dried at 80°C, then transferred to a sintering furnace, heated to 600°C at a rate of 5°C / min, kept warm for 90 minutes, and naturally cooled to obtain pre-sintered bricks.

[0047] S6: Soak the pre-sintered brick blank with a reinforcing treatment agent to a moisture content of 15%, dry at 80°C, then transfer to a sintering furnace, heat to 300°C at a rate of 5°C / min, keep warm for 60 minutes, then heat to 950°C at a rate of 10°C / min, keep warm for 90 minutes, then heat to 1250°C at a rate of 10°C / min, keep warm for 90 minutes, cool naturally to obtain gangue bricks, and complete the preparation method of gangue bricks that fully utilize waste resources.

[0048] Comparative Example 1: Based on Example 3, in step S3, the waste concrete is crushed into particles with a particle size of 5-10 mm, and then directly used as aggregate to replace the pretreated concrete aggregate in step S4 without being treated with graphene oxide treatment liquid. The other steps remain unchanged to prepare coal gangue bricks.

[0049] Comparative Example 2: Based on Example 3, the nanoparticle dispersion in step S2 is used instead of the reinforcing agent, and the other steps remain unchanged to prepare coal gangue bricks.

[0050] Comparative Example 3: Based on Example 3, the aluminum carboxylate sol in step S2 is used instead of the reinforcing agent, and the other steps remain unchanged to prepare coal gangue bricks.

[0051] Performance tests were performed on Examples 1 to 3 and Comparative Examples 1 to 3, and the water permeability coefficient and compressive strength of different samples were tested with reference to GB / T25993-2010. The results are shown in Table 1:

[0052] Table 1

[0053] project Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 <![CDATA[Permeability coefficient (×10 -2 cm / s)]]> 3.87 3.83 3.81 3.85 3.53 3.89 Compressive strength(MPa) 35.6 36.9 37.5 29.2 38.0 32.8

[0054] It can be seen from Table 1 that the gangue bricks in Examples 1 to 3 have higher water permeability and compressive strength. The decrease in compressive strength in Example 1 is due to cracks in ordinary waste concrete aggregate during high-temperature sintering; the decrease in water permeability in Example 2 is due to the decomposition of organic matter in the process of converting carboxylate aluminum sol into alumina, which produces gas and increases the effective porosity; the decrease in compressive strength in Example 3 is due to the fact that no nanoparticle dispersion is added, and the organosilane in the nanoparticle dispersion can be cross-linked under initial heat preservation, thereby increasing the stability of the pre-sintered brick blank. In the subsequent sintering process, the organosiloxane is pyrolyzed to form amorphous ceramics such as silicon carbide, and nano-magnesium oxide and nano-zirconium oxide play a solid solution role, so that a denser ceramic material is formed at the aggregate bonding position.

[0055] It should be noted that, in this article, terms such as "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0056] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing coal gangue bricks that fully utilizes waste resources, characterized in that: The steps include: Step 1: crush the waste concrete into particles with a particle size of 5-10 mm, evenly spray the graphene oxide treatment liquid on the surface of the particles at a ratio of 10 kg: 1 L, and obtain pretreated concrete aggregate after natural drying; Step 2: Mix the gangue coarse aggregate, the gangue fine aggregate, the gangue sand and the pre-treated concrete aggregate, then add clean water and mix evenly, then add kaolin and potassium feldspar, and mix evenly to obtain a mixture; Step 3: Press the mixture into a mold at a pressure of 22-25 kg / cm 2 , drying the obtained brick at 60-80°C, then transferring it to a sintering furnace, heating it to 550-600°C at 3-5°C / min, keeping it at that temperature for 60-90min, and cooling it naturally to obtain a pre-sintered brick; Step 4: soak the pre-sintered brick with a reinforcing treatment agent to a moisture content of 10-15%, dry at 60-80°C, transfer to a sintering furnace, heat to 250-300°C at 3-5°C / min, keep warm for 45-60min, heat to 900-950°C at 5-10°C / min, keep warm for 60-90min, heat to 1200-1250°C at 5-10°C / min, keep warm for 60-90min, cool naturally, and obtain coal gangue bricks that fully utilize waste resources.

2. The method for preparing coal gangue bricks by making full use of waste resources according to claim 1, characterized in that: The particle size of the gangue coarse aggregate is 5-10 mm, the particle size of the gangue fine aggregate is 2-4 mm, the particle size of the gangue sand is less than 0.45 mm, and the particle sizes of kaolin and potassium feldspar are less than 0.2 mm.

3. The method for preparing coal gangue bricks by fully utilizing waste resources according to claim 1, characterized in that: The mass ratio of the gangue coarse aggregate, the gangue fine aggregate, the gangue sand, the pre-treated concrete aggregate, the clean water, the kaolin and the potassium feldspar is 5-10:15-25:45-60:80-120:9-14:6-12:12-18.

4. The method for preparing coal gangue bricks by fully utilizing waste resources according to claim 1, characterized in that: The graphene oxide treatment solution is prepared by the following steps: Graphite and sodium nitrate are added to a reactor, 98wt% concentrated sulfuric acid is added at 0-5°C and stirred for 1.5-2h, potassium permanganate is added and stirred for 7-8h, 70°C hot water is added and stirred for 1.5-2h, 30wt% hydrogen peroxide solution is added and stirred for 1h, the precipitate is allowed to stand and washed and dried to obtain graphene oxide; graphene oxide, hydroxypropyl cellulose and deionized water are added to the reactor in a mass ratio of 1:1:1000, stirred and mixed, and ultrasonically dispersed for 20-30min to obtain a graphene oxide treatment solution.

5. The method for preparing coal gangue bricks by fully utilizing waste resources according to claim 4, characterized in that: The usage ratio of the graphite, sodium nitrate, concentrated sulfuric acid, potassium permanganate, hot water and hydrogen peroxide is 2-4g:1-2g:200-400mL:8-15g:200-400mL:80-100mL.

6. The method for preparing coal gangue bricks by fully utilizing waste resources according to claim 1, characterized in that: The reinforcing treatment agent is prepared by the following steps: Tetramethyltetravinylcyclotetrasiloxane and polymethylhydrogensiloxane are added into a reaction kettle, stirred for 20-30 minutes at 20-25°C and 200-300r / min, and then nano-magnesium oxide powder and nano-zirconium oxide powder are added into the reaction kettle, and stirred for 20-30 minutes to obtain a nano-particle dispersion; aluminum carboxylate sol and the nano-particle dispersion are stirred and mixed at a mass ratio of 5:1 to obtain a reinforcing treatment agent.

7. The method for preparing coal gangue bricks by fully utilizing waste resources according to claim 6, characterized in that: The dosage ratio of tetramethyltetravinylcyclotetrasiloxane, polymethylhydrogensiloxane, nano magnesium oxide powder and nano zirconium oxide powder is 68-70:44-45:5-6:5-6.

8. The method for preparing coal gangue bricks by fully utilizing waste resources according to claim 6, characterized in that: The aluminum carboxylate sol is prepared by the following steps: Deionized water, formic acid and acetic acid are added into a reaction kettle, stirred at 200-300 r / min for 5-10 min, heated to 85-90° C., aluminum powder is added into the reaction kettle, stirring is continued for 2.5-3 h, nitric acid with a mass fraction of 68% is added into the reaction kettle, and the reaction is kept warm for 18-20 h to obtain carboxylate aluminum sol.

9. The method for preparing coal gangue bricks by fully utilizing waste resources according to claim 8, characterized in that: The mass ratio of the deionized water, formic acid, acetic acid, aluminum powder and nitric acid is 500:30:36:27:

32.

10. A coal gangue brick that fully utilizes waste resources, characterized in that: It is prepared by the preparation method described in any one of claims 1 to 9.