Zwitterionic intermediate, chitosan derivative, preparation method and application

By introducing chitosan derivatives modified with imidazolium zwitterionic intermediates, the existing corrosion inhibitor costs, environmental pollution and low corrosion inhibition efficiency are solved, and the corrosion inhibition effect of high efficiency and environmentally friendly metal materials is achieved, especially Highly efficient corrosion-resistant in acidic solutions.

CN119039481APending Publication Date: 2024-11-29QIANNAN NORMAL UNIV FOR NATTIES

Patent Information

Application Number
CN202410928545.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-03-21
Filing Date
2024-07-11
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing organic corrosion inhibitors have problems such as high cost, large environmental pollution, complex preparation process and low corrosion inhibition efficiency in metal corrosion prevention. The existing modified chitosan preparation method uses toxic organic reagents, environmental protection and process flow. Not ideal.

Method used

By introducing imidazolium zwitterionic intermediates, modifying chitosan derivatives (CS-FGA) to improve their adsorption capacity and water solubility on the metal surface, a zwitterionic chitosan derivative is prepared for improving the augmentation capacity and water solubility of the metal surface. Corrosion inhibition efficiency of metal materials.

Benefits of technology

It achieves an efficient corrosion inhibition effect of metal materials, especially the corrosion inhibition efficiency of carbon steel in acidic solutions reaches 99.4%, and it also has an environmentally friendly and simplified preparation process, reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039481A_ABST
    Figure CN119039481A_ABST
Patent Text Reader

Abstract

The invention relates to a zwitterionic intermediate, a chitosan derivative, and a preparation method and application of the zwitterionic intermediate and the chitosan derivative. The preparation method of the chitosan derivative comprises the following steps: mixing ethanediamine, glyoxal, formaldehyde and water, reacting, carrying out solid-liquid separation, and carrying out alcohol washing to obtain a zwitterionic intermediate FGA; and mixing chitosan, a dissolution promoter and water, stirring at 50-60 DEG C for 4-6 hours, adding the zwitterionic intermediate FGA and a protective agent, reacting at 30-120 DEG C for 4-48 hours, recovering a crude product, and purifying to obtain the chitosan derivative. The chitosan derivative disclosed by the invention has high corrosion inhibition efficiency and dissolving property, and has a relatively good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of energy conservation and environmental protection, and in particular to a corrosion inhibitor and a preparation method and application thereof. Background Art

[0002] Metal materials have the characteristics of good toughness, high thermal conductivity, easy manufacturing, outstanding fatigue resistance and low cost. With the rapid development of the manufacturing industry, the demand for metal materials is growing rapidly. However, metals are more susceptible to corrosion in the natural environment, which causes a series of problems. In order to solve the above problems, researchers have currently developed relevant strategies to inhibit the corrosion of metal materials, such as coatings, cathodic protection and corrosion inhibitors.

[0003] The application of corrosion inhibitors is considered to be one of the most effective metal corrosion protection technologies. As one of the most common corrosion inhibitors, organic corrosion inhibitors have attracted widespread attention. In recent years, material researchers have been working hard to study new and efficient organic corrosion inhibitors. However, most organic corrosion inhibitors have disadvantages such as high cost, large environmental pollution, and complex preparation processes, which seriously limit their application in practice. Therefore, from the perspective of green chemistry, it is urgent to develop a non-toxic, biodegradable, and biocompatible corrosion inhibitor. At present, studies have shown that some natural compounds (amino acids, plant extracts, natural polymers, etc.) have good corrosion inhibition effects on metals. At the same time, these compounds are easy to obtain and environmentally friendly, so they are all potential corrosion inhibitors. But they show a common feature, that is, low corrosion inhibition efficiency. Therefore, it is urgent to modify these compounds to improve the corrosion inhibition efficiency. Therefore, it is of great significance to develop a corrosion inhibitor that is environmentally friendly, has high corrosion inhibition efficiency, and has low toxicity in a corrosive medium environment.

[0004] Chitosan is obtained by deacetylation of chitin, which is widely found in nature. Its chemical name is polyglucosamine (1-4)-2-amino-BD glucose. It is often used as a corrosion inhibitor for metal materials, but its water solubility and corrosion inhibition effect are poor. Therefore, the existing technology usually modifies it and uses it as a corrosion inhibitor.

[0005] Chinese invention patent application CN117603373A discloses a method for preparing a high-temperature resistant CO2 modified chitosan corrosion inhibitor, comprising the following steps: adding potassium hydroxide to a flask containing DMF, stirring until dissolved, then adding 1,2-dichloroethane, and heating and stirring. Dissolve 2-methylimidazole in DMF, add dropwise to the flask, and stir at a constant temperature. After the reaction is completed, filter and rotary evaporate to obtain an intermediate product; add potassium carbonate to a flask containing DMF, stir until dissolved, then add chitosan, and heat and stir. Dissolve the intermediate product in DMF, add dropwise to the flask, and stir at a constant temperature. After the reaction is completed, filter and rotary evaporate to obtain a modified chitosan corrosion inhibitor. The preparation process of this invention requires the use of toxic or carcinogenic organic reagents such as DMF, 2-methylimidazole, and 1,2-dichloroethane, and its environmental protection needs to be improved, and the preparation process is relatively long. Summary of the invention

[0006] One of the purposes of the present invention is to provide a chitosan derivative (CS-FGA) with high corrosion inhibition efficiency in view of the shortcomings of the prior art; the second purpose of the present invention is to provide a zwitterionic intermediate; the third purpose of the present invention is a method for preparing a chitosan derivative; the fourth purpose of the present invention is to provide the use of a chitosan derivative as a sustained-release agent for metal materials.

[0007] In order to solve the above technical problems, the technical solution of the present invention is as follows:

[0008] A chitosan derivative, whose chemical structural formula is shown in Formula 1:

[0009]

[0010] Wherein R1 is selected from -NH2;

[0011] R2 is selected from -NH2;

[0012] The chitosan derivative The number of is 1 to 2n;

[0013] The R1 of each repeating unit of the chitosan derivative is the same or different; the R2 of each repeating unit of the chitosan derivative is the same or different;

[0014] n is an integer from 30-200, preferably 50-190, more preferably 100-185.

[0015] Furthermore, the chemical structural formula of the chitosan derivative is as shown below:

[0016]

[0017] A zwitterionic intermediate, the chemical structure of which is shown below:

[0018]

[0019] The method for preparing the chitosan derivative as described above comprises the following steps:

[0020] S1, mixing amino acid, glyoxal, low carbon aldehyde and water, reacting, separating solid from liquid, washing with alcohol, and obtaining zwitterionic intermediate FGA;

[0021] S2. Mix chitosan, a dissolving agent and water, stir at 50-60° C. for 4-6 hours, add the zwitterionic intermediate FGA and a protective agent, react at 30-90° C. (preferably 50-80° C.) for 4-48 hours, recover the crude product, purify it, and obtain a chitosan derivative.

[0022] Furthermore, in S1, the molar ratio of amino acid, glyoxal and low-carbon aldehyde is 2-5:2.5-5:1-3, preferably 2.5-4.5:3-4.5:1.5-2.5.

[0023] Further, in S1, the mass ratio of tyrosine amino acid, glyoxal, and formaldehyde low-carbon aldehyde is 1-10:1-10:1, preferably 5-6:5-6:1;

[0024] Preferably, the mass ratio of the amino acid tyrosine, glyoxal, low carbon aldehyde formaldehyde (without using other aldehydes) and water is 1-10:1-10:1:10-50, preferably 5-6:5-6:1:20-40.

[0025] Furthermore, in S1, the reaction temperature is 35-85°C, preferably 55-65°C; the reaction time is 4-24h, preferably 8-12h; preferably, the solid-liquid separation method is suction filtration.

[0026] Furthermore, in S1, saturated fatty alcohol is used for alcohol washing, preferably, the molecular weight of the saturated fatty alcohol is less than 200; more preferably, the saturated fatty alcohol includes one or more of methanol, ethanol, propanol and butanol.

[0027] Preferably, the amino acid is one or more of tyrosine, alanine and butyraldehyde; the low-carbon aldehyde is one or more of formaldehyde, acetaldehyde, propionaldehyde and butyraldehyde.

[0028] Further, in S2, the mass ratio of chitosan and zwitterionic intermediate FGA is 1-3:1-5;

[0029] Preferably, the mass ratio of chitosan to the solubilizing agent is 2:0.5-2, preferably 2:0.75-1.25. Preferably, the solubilizing agent includes one or more of N-hydroxysuccinimide, N-hydroxymethyl acrylamide, and vinylguanamine;

[0030] Preferably, the mass ratio of chitosan, dissolution agent and water is 2:0.5-2:1-2, more preferably 2:0.75-1.75:1.25-1.75;

[0031] Preferably, the mass ratio of the added zwitterionic intermediate FGA to the protective agent is 2:0.5-2, preferably 2:0.75-1.25. Preferably, the protective agent includes one or more of ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride.

[0032] Furthermore, in S2, the weight average molecular weight of chitosan is 6000-60000, preferably 7000-55000, and preferably 8000-20000.

[0033] Furthermore, in S2, the reaction temperature is 55-65°C; and the reaction time is 24-36h.

[0034] Furthermore, the purification method is dialysis. Preferably, the crude product is loaded into a dialysis bag, and deionized water is used as a dialysis agent, and dialyzed at 15-45° C. for 10-84 hours.

[0035] Application of the chitosan derivative as described above or the chitosan derivative prepared by the preparation method in corrosion protection of metal materials.

[0036] Furthermore, the chitosan derivative as described above or the chitosan derivative prepared by the preparation method described above is used to reduce the corrosion rate of carbon steel in an acidic solution environment.

[0037] Optionally, the metal material is steel, and further is carbon steel.

[0038] Furthermore, the concentration of the chitosan derivative in the acidic solution is 50-1000 mg / L, preferably 100-600 mg / L.

[0039] In the preparation method of the chitosan derivative (CS-FGA) of the present invention, ethylamine, glyoxal and formaldehyde are first used as raw materials to synthesize an imidazolium zwitterionic intermediate, and then, the C=O group of the imidazolium zwitterionic intermediate reacts with -NH2 in chitosan to finally obtain a zwitterionic chitosan derivative (CS-FGA), so that the chitosan derivative has excellent corrosion inhibition performance and is easily soluble in water.

[0040] The introduction of the imidazolium zwitterionic intermediate in the present invention can provide multiple adsorption active sites, such as cations, N elements, carboxyl groups and other adsorption active sites, thereby effectively promoting the adsorption of chitosan derivatives (CS-FGA) on the metal surface and improving the corrosion inhibition efficiency.

[0041] The invention uses natural product chitosan (CS) as raw material and introduces imidazolium zwitterion intermediate (FGA) to synthesize a chitosan derivative (CS-FGA) with high corrosion inhibition efficiency and environmental protection. The chitosan derivative has a corrosion inhibition efficiency of up to 99.4% for carbon steel in 0.5MH2SO4 solution.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] (1) The raw material chitosan (CS) used in the present invention is highly environmentally friendly.

[0044] (2) The present invention introduces an imidazolium zwitterionic intermediate to make the chitosan derivative (CS-FGA) have more active adsorption sites, thereby improving the corrosion inhibition performance of the chitosan derivative;

[0045] (3) The chitosan derivative (CS-FGA) of the present invention is a green and environmentally friendly corrosion inhibitor, and its corrosion inhibition efficiency for carbon steel in 0.5MH2SO4 solution is as high as 99.4%, with good corrosion inhibition effect.

[0046] (4) The present invention uses -NH2 of chitosan itself as the modification site and grafts FGA onto chitosan through amide reaction, which makes the reaction process easier and helps to reduce the preparation cost.

[0047] (5) The chitosan derivative of the present invention also has good solubility and can be well dissolved in water, which is conducive to industrial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 : Fourier transform infrared (FT-IR) spectrum of the chitosan derivative (CS-FGA) sample obtained in Example 1.

[0049] Figure 2 : Example 1 obtained chitosan derivative (CS-FGA) sample and chitosan (CS) sample of hydrogen nuclear magnetic resonance ( 1 HNMR) spectrum.

[0050] Figure 3: Open circuit potential (OCP) curves of carbon steel after being immersed in 0.5M H2SO4 solution (blank sample) and 0.5M H2SO4 mixed solution containing 500 mg / L CS-FGA, 0.5M H2SO4 mixed solution containing 500 mg / L CS-FGA1, and 0.5MH2SO4 mixed solution containing 500 mg / L CS-FGA2 for 24 hours.

[0051] Figure 4 : Potentiodynamic polarization curves of carbon steel after being immersed in 0.5M H2SO4 solution (blank sample) and 0.5M H2SO4 mixed solution containing 500 mg / L CS-FGA, 0.5M H2SO4 mixed solution containing 500 mg / L CS-FGA1, and 0.5MH2SO4 mixed solution containing 500 mg / L CS-FGA2 for 24 hours.

[0052] Figure 5 : Nyquist curve of carbon steel after being immersed in 0.5M H2SO4 solution (blank sample) and 0.5M H2SO4 mixed solution containing 500 mg / L CS-FGA, 0.5M H2SO4 mixed solution containing 500 mg / L CS-FGA1, and 0.5MH2SO4 mixed solution containing 500 mg / L CS-FGA2 for 24 hours. DETAILED DESCRIPTION

[0053] The present invention will be described in detail below in conjunction with the embodiments. It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present invention can be combined with each other. Unless otherwise specified, the relevant percentages refer to mass percentages.

[0054] Example 1

[0055] The preparation method of the chitosan derivative (CS-FGA) of this embodiment is as follows:

[0056] S1. Weigh 50 mg of ethylamine, 50 mg of glyoxal and 10 mg of formaldehyde into a 250 mL round-bottom flask, add 200 mL of deionized water, turn on magnetic stirring, and after all the substances are dissolved, react at 65 ° C for 12 h, vacuum filter, collect the filtrate, and wash it with anhydrous ethanol 3-4 times to obtain the imidazolium zwitterionic intermediate FGA for standby use.

[0057] S2. Weigh 200 mg of chitosan with a weight average molecular weight of 50,000 and 100 mg of N-hydroxysuccinimide, add them to a round-bottom flask filled with 200 mL of deionized water, stir magnetically, and after all the substances are dissolved, adjust the reaction temperature to 60°C. After reacting for 6 hours, add 100 mg of the above-prepared imidazolium zwitterion intermediate FGA and 50 mg of ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride to the reaction system, then react at 65°C for 36 hours. After the reaction is completed, recover to obtain a crude CS-FGA product.

[0058] S3. The crude CS-FGA product was loaded into a dialysis bag, and deionized water was used as a dialyzer. The dialysis was performed at 30° C. for 48 h to finally obtain a pure CS-FGA product.

[0059] 10 mg of the prepared CS-FGA and CS were taken respectively and characterized by infrared spectrometer and nuclear magnetic resonance. The results are as follows: Figure 1 and Figure 2 shown.

[0060] Figure 1 This is the Fourier transform infrared (FT-IR) spectrum of CS-FGA. -1 To 3400cm -1 The absorption peaks between are the stretching vibration peaks of NH and OH, 2903.1cm -1 The absorption peak at 1629.5 cm is the stretching vibration peak of -CH -1 The absorption peaks are divided into the stretching vibration peak of -C=N, 1520.0cm -1 The absorption peak at 1055.3cm is the stretching vibration peak of C=C. -1 The absorption peak is that of polysaccharide monomer.

[0061] Figure 2 The H NMR of CS-FGA and CS ( 1 H NMR) spectrum. The chemical shifts at 3.2-4.8 ppm are the protons of the glucosamine unit, and the chemical shift at 1.85 ppm is the residual methyl proton of the N-acetyl group. Compared with CS, the intensity of the chemical shift at 1.85 ppm of CS-FGA is significantly reduced, which is attributed to the amidation reaction between -NH2 of CS and -COOH of FGA. In CS-FGA, the chemical shift at 7.28 ppm is the proton of CH=N in the Schiff base, and the chemical shift at 6.75-7.05 ppm is the proton of the heterocyclic group.

[0062] Example 2

[0063] The preparation method of the chitosan derivative (CS-FGA-1) of this embodiment is as follows:

[0064] S1. Weigh 100 mg of ethylamine, 100 mg of glyoxal and 10 mg of formaldehyde into a 250 mL round-bottom flask, add 200 mL of deionized water, start magnetic stirring, and after all the substances are dissolved, react at 55 °C for 12 h. After the reaction is completed, vacuum filter, collect the filtrate, and wash it with anhydrous ethanol for 3-4 times to obtain the imidazolium zwitterion intermediate FGA-1 for standby use.

[0065] S2. Weigh 200 mg of chitosan with a weight average molecular weight of 50,000 and 100 mg of N-hydroxymethyl acrylamide, add them into a round-bottom flask filled with 200 mL of deionized water, stir magnetically, and after all the substances are dissolved, adjust the reaction temperature to 60°C and react for 6 hours; after the reaction, add 100 mg of the above-prepared imidazolium zwitterion intermediate FGA-1 and 50 mg of ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride to the reaction system, then react at 65°C for 36 hours. After the reaction, recover to obtain a crude product of CS-FGA-1.

[0066] S3. Load the crude CS-FGA-1 product into a dialysis bag, use deionized water as a dialysis agent, and dialyze at 30° C. for 48 h to finally obtain a pure CS-FGA-1 product.

[0067] Example 3

[0068] The preparation method of the chitosan derivative (CS-FGA-2) of this embodiment is as follows:

[0069] S1. Weigh 60 mg of ethylamine, 60 mg of glyoxal and 10 mg of formaldehyde into a 250 mL round-bottom flask, add 200 mL of deionized water, turn on magnetic stirring, and after all the substances are dissolved, react at 60 ° C for 12 h; after the reaction is completed, vacuum filter, collect the filtrate, and wash it with butanol 3-4 times to obtain the imidazolium zwitterion intermediate FGA-2 for standby use.

[0070] S2. Weigh 200 mg of chitosan with a weight average molecular weight of 60,000 and 100 mg of N-hydroxymethyl acrylamide, add them to a round-bottom flask containing 200 mL of deionized water, stir magnetically, and after all the substances are dissolved, adjust the reaction temperature to 60°C and react for 6 hours; after the reaction, add 100 mg of the intermediate FGA-2 prepared above and 50 mg of ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride to the reaction system, then react at 65°C for 36 hours. After the reaction, recover and obtain the crude product of CS-FGA-2.

[0071] S3. Load the crude CS-FGA-2 product into a dialysis bag, use deionized water as a dialysis agent, and dialyze at 30° C. for 48 hours to finally obtain a pure CS-FGA-2 product.

[0072] The solubility of CS-FGA, CS-FGA-1 and CS-FGA-2 in water was tested, and the results were 1.12S (i.e. g / 100g water), 1.11S and 1.12S respectively, all showing good water solubility.

[0073] Cut Q325 carbon steel with a size of 2 cm × 2 cm, and use 300 mesh, 600 mesh, 800 mesh, 1200 mesh and 1500 mesh sandpaper to grind the surface of the carbon steel in turn, and then clean it with deionized water, anhydrous ethanol and acetone in turn under the action of ultrasound, dry it in a vacuum state, and set it aside;

[0074] The four pieces of carbon steel treated as above were immersed in 0.5M H2SO4 solution (blank sample), 0.5M H2SO4 mixed solution containing 500 mg / L CS-FGA, 0.5M H2SO4 mixed solution containing 500 mg / L CS-FGA-1, and 0.5M H2SO4 mixed solution containing 500 mg / L CS-FGA-2 for 24 hours, and the solution temperature was controlled at 25°C; after the immersion, the corresponding carbon steel was taken out, blown dry with N2, and set aside. The measurement adopts the classic three-electrode system, with the carbon steel to be used as the working electrode, the Pt electrode as the auxiliary electrode, and the reference electrode as a saturated calomel electrode. The open circuit potential, electrochemical impedance spectrum (EIS) and potentiodynamic polarization curve of carbon steel in different corrosion inhibitor solutions were tested respectively, and the results are as follows Figure 3 , Figure 4 as well as Figure 5 shown.

[0075] Figure 3 The open circuit potential (OCP) curves of carbon steel after being immersed in 0.5M H2SO4 solution (blank sample), 0.5M H2SO4 mixed solution containing 500 mg / L CS-FGA, 0.5M H2SO4 mixed solution containing 500 mg / L CS-FGA-1, and 0.5M H2SO4 mixed solution containing 500 mg / L CS-FGA-2 for 24 hours. It can be found that compared with the blank control sample, the corresponding open circuit potential value of carbon steel in the H2SO4 solution containing CS-FGA, CS-FGA-1 and CS-FGA-2 samples moves to the negative direction, which shows that CS-FGA, CS-FGA-1 and CS-FGA-2 can be better adsorbed on the surface of carbon steel to replace the water molecules previously adsorbed on the surface of carbon steel, thereby forming a protective film on the surface of carbon steel to prevent carbon steel from being corroded.

[0076] Figure 4The potentiodynamic polarization curves of carbon steel after being immersed in 0.5M H2SO4 solution (blank sample), 0.5M H2SO4 mixed solution containing 500 mg / L CS-FGA, 0.5M H2SO4 mixed solution containing 500 mg / L CS-FGA-1, and 0.5M H2SO4 mixed solution containing 500 mg / L CS-FGA-2 for 24 hours. It can be found that compared with the blank control sample, when the H2SO4 solution contains CS-FGA, CS-FGA-1 and CS-FGA-2, the corrosion potential of carbon steel is reduced, and the corrosion current density is 0.196μA cm -2 , 0.209μA cm -2 and 0.202 μA cm -2 , while the corrosion current density of the blank sample is 32.6 μA cm -2 Using the corrosion current density, the corrosion inhibition efficiency (η i ):

[0077]

[0078] Among them, i corr(0) and i corr(inh) They are the current density of the blank sample and the current density of the sample with corrosion inhibitor added. After calculation, the corrosion inhibition efficiencies of CS-FGA, CS-FGA-1 and CS-FGA-2 are 99.40%, 99.36% and 99.38% respectively.

[0079] Figure 5 Nyquist curves of carbon steel after being immersed in 0.5M H2SO4 solution (blank sample), 0.5M H2SO4 mixed solution containing 500 mg / L CS-FGA, 0.5M H2SO4 mixed solution containing 500 mg / L CS-FGA-1, and 0.5M H2SO4 mixed solution containing 500 mg / L CS-FGA-2 for 24 hours. Figure 5 It is a semicircular arc compressed on the Y axis. The radius of the X axis arc can reflect the corrosion inhibition efficiency of the sample. Generally, the larger the radius, the greater the transfer charge (Rct) between the solution and the carbon steel interface, and thus the higher the corrosion inhibition efficiency; on the contrary, if the radius is smaller, the corrosion inhibition efficiency is lower. Compared with the blank sample, the X axis arc radius of CS-FGA, CS-FGA-1 and CS-FGA-2 is much larger, and the Rct values ​​of CS-FGA, CS-FGA-1 and CS-FGA-2 are 2187.2Ωcm respectively. 2 、2111.6Ωcm 2 、2048.6Ωcm 2 (much higher than the Rct value of the blank sample 12.7Ωcm 2). Using Rct, the corrosion inhibition efficiency (η R %):

[0080]

[0081] Among them, R (inh) and R (0) The Rct values ​​with and without corrosion inhibitors are shown in Table 1. After calculation, the corrosion inhibition efficiencies of CS-FGA, CS-FGA-1, and CS-FGA-2 are 99.42%, 99.4%, and 99.38%, respectively.

[0082] Example 4

[0083] The preparation method of the chitosan derivative (CS-FGA-3) of this embodiment is as follows:

[0084] S1. Weigh 60 mg of ethylamine, 60 mg of glyoxal and 10 mg of formaldehyde into a 250 mL round-bottom flask, add 200 mL of deionized water, turn on magnetic stirring, and react at 55 °C for 8 h after all the substances are dissolved. After the reaction is completed, vacuum filter, collect the filtrate, and wash it with butanol 3-4 times to obtain the imidazolium zwitterionic intermediate FGA-3 for standby use.

[0085] S2. Weigh 200 mg of chitosan with a weight average molecular weight of 50,000 and 100 mg of N-hydroxymethyl acrylamide, add them to a round-bottom flask containing 200 mL of deionized water, stir magnetically, and after all the substances are dissolved, adjust the reaction temperature to 60°C and react for 6 hours; after the reaction, add 100 mg of the intermediate FGA-3 prepared above and 50 mg of ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride to the reaction system, then react at 65°C for 36 hours. After the reaction, recover and obtain a crude product of CS-FGA-3.

[0086] S3. Load the crude CS-FGA-3 product into a dialysis bag, use deionized water as a dialyzer, and dialyze at 30° C. for 48 h to finally obtain a pure CS-FGA-3 product.

[0087] The corrosion inhibition efficiency of CS-FGA-3 was measured to be 92.5% using the potentiodynamic polarization curve described above.

[0088] Comparative Example 1

[0089] Example 1 was repeated, except that no N-hydroxysuccinimide was added to S2.

[0090] The corrosion inhibition efficiency of the obtained product measured by the potentiodynamic polarization curve described above was only 80.1%.

[0091] Comparative Example 2

[0092] Example 1 was repeated, except that ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride was not added to S2.

[0093] The corrosion inhibition efficiency of the obtained product measured by the potentiodynamic polarization curve described above was only 83.7%.

[0094] Comparative Example 3

[0095] The preparation method of the chitosan derivative (CS-FGA-4) of this comparative example is as follows:

[0096] S1. Weigh 50 mg of ethylamine, 50 mg of glyoxal and 10 mg of formaldehyde into a 250 mL round-bottom flask, add 200 mL of deionized water, turn on magnetic stirring, and react at 65 °C for 12 h after all the substances are dissolved. After the reaction is completed, vacuum filter, collect the filtrate, and wash it with anhydrous ethanol for 3-4 times to obtain the imidazolium zwitterionic intermediate FGA-4 for standby use.

[0097] S2. Weigh 200 mg of chitosan with a weight average molecular weight of 50,000 and 100 mg of N-hydroxysuccinimide, add them to a round-bottom flask containing 200 mL of deionized water, stir magnetically, and after all the substances are dissolved, adjust the reaction temperature to 60°C and react for 6 hours. After the reaction, add 100 mg of the intermediate FGA-4 prepared above and 50 mg of ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride to the reaction system, then react at 95°C for 48 hours. After the reaction, recover and obtain a crude product of CS-FGA-4.

[0098] S3. Load the crude CS-FGA-4 product into a dialysis bag, use deionized water as a dialysis agent, and dialyze at 30° C. for 48 h to finally obtain a pure CS-FGA-4 product.

[0099] The corrosion inhibition efficiency of CS-FGA-4 was measured to be 84.1% using the potentiodynamic polarization curve described above.

[0100] Comparative Example 4

[0101] The preparation method of the chitosan derivative (CS-FGA-5) of this comparative example is as follows:

[0102] S1. Weigh 50 mg of ethylamine, 50 mg of glyoxal and 10 mg of formaldehyde into a 250 mL round-bottom flask, add 200 mL of deionized water, turn on magnetic stirring, and react at 65 °C for 12 h after all the substances are dissolved. After the reaction is completed, vacuum filter, collect the filtrate, and wash it with anhydrous ethanol for 3-4 times to obtain the imidazolium zwitterionic intermediate FGA-5 for standby use.

[0103] S2. Weigh 200 mg of chitosan with a weight average molecular weight of 50,000 and add it to a round-bottom flask containing 200 mL of deionized water. Stir magnetically. After the substance is completely dissolved, adjust the reaction temperature to 60°C and react for 6 hours. After the reaction, add 100 mg of the intermediate FGA-5 prepared above to the reaction system, and then react at 65°C for 36 hours. After the reaction is completed, recover and obtain a crude product of CS-FGA-5.

[0104] S3. Load the crude CS-FGA-5 product into a dialysis bag, use deionized water as a dialysis agent, and dialyze at 30° C. for 48 hours to finally obtain a pure CS-FGA-5 product.

[0105] The corrosion inhibition efficiency of CS-FGA-5 was measured to be 62.7% using the potentiodynamic polarization curve described above.

[0106] Comparative Example 5

[0107] Example 1 was repeated, except that the zwitterionic intermediate FGA and the protective agent were added to S2, and the reaction was carried out at 25°C.

[0108] As a result, the corrosion inhibition efficiency of the final product measured by the potentiodynamic polarization curve described above was only 71.1%.

[0109] Example 5

[0110] Example 1 was repeated, except that the zwitterionic intermediate FGA and the protective agent were added to S2, and the reaction was carried out at 30°C.

[0111] As a result, the corrosion inhibition efficiency of the final product was measured to be 88.3% using the potentiodynamic polarization curve described above.

[0112] Example 6

[0113] Example 1 was repeated, except that the zwitterionic intermediate FGA and the protective agent were added to S2, and the reaction was carried out at 120°C.

[0114] As a result, the corrosion inhibition efficiency of the final product was measured to be 91.3% using the potentiodynamic polarization curve described above.

[0115] Comparative Example 6

[0116] Example 1 was repeated, except that the zwitterionic intermediate FGA and the protective agent were added to S2, and the reaction was carried out at 125°C.

[0117] As a result, the corrosion inhibition efficiency of the final product was measured to be 86.5% using the potentiodynamic polarization curve described above.

[0118] Comparative Example 7

[0119] Example 1 was repeated, except that the reaction in S1 was carried out at 25°C.

[0120] As a result, the corrosion inhibition efficiency of the final product was measured to be 67.5% using the potentiodynamic polarization curve described above.

[0121] Example 7

[0122] Example 1 was repeated, except that the reaction in S1 was carried out at 35°C.

[0123] As a result, the corrosion inhibition efficiency of the final product was measured to be 88.3% using the potentiodynamic polarization curve described above.

[0124] Example 8

[0125] Example 1 was repeated, except that the reaction in S1 was carried out at 85°C.

[0126] As a result, the corrosion inhibition efficiency of the final product was measured to be 90.6% using the potentiodynamic polarization curve described above.

[0127] Comparative Example 8

[0128] Example 1 was repeated, except that the reaction in S1 was carried out at 90°C.

[0129] As a result, the corrosion inhibition efficiency of the final product was measured to be 85.1% using the potentiodynamic polarization curve described above.

[0130] Comparative Example 9

[0131] Example 1 was repeated, except that the amount of glyoxal added in S1 was 3 mg.

[0132] As a result, the corrosion inhibition efficiency of the final product was measured to be 70.7% using the potentiodynamic polarization curve described above.

[0133] Comparative Example 10

[0134] Example 1 was repeated, except that the amount of glyoxal added in S1 was 4 mg.

[0135] As a result, the corrosion inhibition efficiency of the final product was measured to be 73.8% using the potentiodynamic polarization curve described above.

[0136] Comparative Example 11

[0137] Example 1 was repeated, except that the amount of glyoxal added in S1 was 110 mg.

[0138] As a result, the corrosion inhibition efficiency of the final product was measured to be 73.8% using the potentiodynamic polarization curve described above.

[0139] Example 9

[0140] Example 1 was repeated, except that the amount of glyoxal added in S1 was 100 mg.

[0141] As a result, the corrosion inhibition efficiency of the final product was measured to be 86.2% using the potentiodynamic polarization curve described above.

[0142] Comparative Example 12

[0143] Example 1 was repeated, except that the amount of glyoxal added in S1 was 105 mg.

[0144] As a result, the corrosion inhibition efficiency of the final product was measured to be 72.6% using the potentiodynamic polarization curve described above.

Claims

1. A chitosan derivative, characterized in that: Its chemical structural formula is shown in Formula 1: Wherein R1 is selected from -NH2; R2 is selected from -NH2; The chitosan derivative The number of is 1 to 2n; The R1 of each repeating unit of the chitosan derivative is the same or different; the R2 of each repeating unit of the chitosan derivative is the same or different; n is an integer ranging from 30 to 200.

2. The chitosan derivative according to claim 1, characterized in that The chemical structural formula of the chitosan derivative is shown below:

3. A zwitterionic intermediate, characterized in that: Its chemical structure is shown below:

4. The method for preparing a chitosan derivative according to claim 1 or 2, characterized in that: The following steps are involved: S1, mixing amino acid, glyoxal, low carbon aldehyde and water, reacting, separating solid from liquid, washing with alcohol, and obtaining zwitterionic intermediate FGA; Preferably, the amino acid is one or more of tyrosine, alanine, and butyraldehyde; the low-carbon aldehyde is one or more of formaldehyde, acetaldehyde, propionaldehyde, and butyraldehyde; S2. Mix chitosan, a dissolving agent and water, stir at 50-60° C. for 4-6 hours, add the zwitterionic intermediate FGA and a protective agent, react at 30-90° C. for 4-48 hours, recover the crude product, purify it, and obtain a chitosan derivative.

5. The method for preparing a chitosan derivative according to claim 4, characterized in that: In S1, the mass ratio of amino acid, glyoxal and low carbon aldehyde is 1-10:1-10:1, preferably 5-6:5-6:1; Preferably, the mass ratio of amino acid, glyoxal, low carbon aldehyde and water is 1-10:1-10:1:10-50, preferably 5-6:5-6:1:20-40; Preferably, in S1, the reaction temperature is 35-85°C, preferably 55-65°C; the reaction time is 4-24h, preferably 8-12h; preferably, the solid-liquid separation method is suction filtration.

6. The method for preparing the chitosan derivative according to claim 4, characterized in that: In S1, saturated fatty alcohol is used for alcohol washing. Preferably, the molecular weight of the saturated fatty alcohol is less than 200; more preferably, the saturated fatty alcohol includes one or more of methanol, ethanol, propanol and butanol.

7. The method for preparing a chitosan derivative according to claim 4, characterized in that: In S2, the mass ratio of chitosan and zwitterionic intermediate FGA is 1-3:1-5; Preferably, the mass ratio of chitosan to the solubilizing agent is 2:0.5-2. Preferably, the solubilizing agent comprises one or more of N-hydroxysuccinimide, N-hydroxymethyl acrylamide, and vinylguanamine; Preferably, the mass ratio of chitosan, dissolution agent and water is 2:0.5-2:1-2, more preferably 2:0.75-1.75:1.25-1.75; Preferably, the mass ratio of the added zwitterionic intermediate FGA to the protective agent is 2:0.5-2, and preferably, the protective agent includes one or more of ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride; Preferably, the weight average molecular weight of chitosan is 6000-60000, more preferably 8000-20000.

8. The method for preparing a chitosan derivative according to claim 4, characterized in that: The purification method is dialysis. Preferably, the crude product is loaded into a dialysis bag, and deionized water is used as a dialysis agent, and dialyzed at 15-45° C. for 10-84 hours.

9. The method for preparing a chitosan derivative according to claim 4, characterized in that: In S2, the reaction temperature is 55-65°C; the reaction time is 24-36h.

10. Use of the chitosan derivative according to claim 1 or 2 or the chitosan derivative prepared by the preparation method according to any one of claims 3 to 9 in corrosion protection of metal materials.

Citation Information

Patent Citations

  • Preparation method and application of high-temperature-resistant CO2 modified chitosan corrosion inhibitor

    CN117603373A

Cited By

  • Chitosan oligosaccharide zwitterionic corrosion inhibitor containing long-chain structure as well as preparation method and application of chitosan oligosaccharide zwitterionic corrosion inhibitor

    CN122060006A

  • Chitosan oligosaccharide zwitterionic corrosion inhibitor containing long chain structure, preparation method and application