Protein adsorption resistant TPE (Thermoplastic Elastomer) material and preparation method thereof

Through the ratio of components such as SEBS, mineral oil, polypropylene and twin screw extrusion processes, TPE materials with anti-protein adsorption properties were prepared, which solved the problems of anti-pollution and poor anti-protein adsorption properties of existing TPE materials, and achieved Good sealing barrier and mechanical properties in the field of in vitro diagnostic and medical consumables.

CN119039794APending Publication Date: 2024-11-29DONGGUAN GUYUAN MEDICAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411053274.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing TPE materials have poor anti-contamination and protein adsorption performance in the field of in vitro diagnostic or medical consumables, and are prone to adsorbing reagents, affecting the test results.

Method used

Using the ratio of components such as SEBS, mineral oil, polypropylene, filler, hydrophilic additive and antioxidant, melt-kneading, extrusion and granulation through a twin-screw extruder to prepare a protein adsorption resistance. TPE material.

Benefits of technology

It improves the protein adsorption and sealing barrier properties of TPE materials, which are better than the silicone plug materials on the market, and are suitable for in vitro diagnostic and medical consumables, and uses low-cost raw materials, which is safe and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004975557110000061
    Figure BDA0004975557110000061
Patent Text Reader

Abstract

The invention discloses a protein adsorption resistant TPE material and a preparation method thereof, the protein adsorption resistant TPE material comprises the following raw materials by weight: 10-40 parts of SEBS, 30-50 parts of mineral oil, 10-40 parts of polypropylene, 5-20 parts of a filler, 1-5 parts of a hydrophilic auxiliary agent, 0.1-1 part of an antioxidant and 0.1-1 part of a dispersant. The invention has the following beneficial effects: the material has high sealing property and barrier property, and can effectively prevent a reagent from volatilizing; by adding PP, physical crosslinking points of a composite system can be increased, so that the mechanical property of SEBS is improved, the permanent deformation resistance and creep resistance of the material are enhanced, and different application requirements can be met by adjusting parameters such as the ratio of basic raw materials and the process; in addition, by adding the hydrophilic aid, the material is endowed with better protein adsorption resistance, and the used materials are all safe and environment-friendly raw materials and have a larger application prospect in the field of in-vitro diagnosis or medical consumables.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of TPE material products, and in particular to a protein adsorption resistant TPE material and a preparation method thereof. Background Art

[0002] TPE is a styrene-based thermoplastic elastomer material that combines the high elasticity of rubber with the easy processing properties of plastic. It has many advantages such as environmental protection and non-toxicity, excellent colorability, wide hardness range, weather resistance, soft touch, fatigue resistance, temperature resistance, etc. It has excellent processing performance and does not require vulcanization, and can be recycled, effectively reducing the cost of use.

[0003] With the progress of society and the rapid development of economy, TPE is widely used in our daily life, such as in vitro diagnostics, medical consumables, furniture and kitchenware, toys, sports and health. In recent years, in vitro diagnostics (IVD) has been developing continuously, and the demand for plastic products for containing reagents (such as proteins, enzymes, etc.) has been increasing. Silicone is one of the commonly used materials for reagent bottle stoppers, and the cost is relatively high. In addition, it is formed by vulcanization process, and the molding process is complicated. The product has high water absorption and air permeability. When used as a reagent bottle stopper material, it is easy to cause poor sealing, reagent concentration and volume changes, etc.

[0004] TPE material is one of the best materials to replace traditional rubber as reagent bottle stopper material. It can meet the needs of this market segment in terms of sealing barrier, environmental recycling and cost.

[0005] In the prior art, TPE has poor anti-pollution and anti-protein adsorption properties. When used in the field of in vitro diagnosis or medical consumables, it is easy to adsorb reagents, thereby affecting the test results. Summary of the invention

[0006] The purpose of the present invention is to provide a protein adsorption resistant TPE material and a preparation method thereof, so as to prepare a TPE material with protein adsorption resistance using low-cost raw materials, so as to solve the problems raised in the above-mentioned background technology.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] A protein adsorption resistant TPE material comprises, by weight, 10-40 parts of SEBS, 30-50 parts of mineral oil, 10-40 parts of polypropylene, 5-20 parts of filler, 1-5 parts of hydrophilic additive, 0.1-1 parts of antioxidant and 0.1-1 parts of dispersant.

[0009] As a preferred embodiment of the present invention, the SEBS is a linear block copolymer with an ethylene-butene copolymer obtained by hydrogenating polybutadiene as a middle elastic block.

[0010] As a preferred embodiment of the present invention: the mineral oil is paraffin-based white oil, the flash point of the mineral oil is ≥ 200°C, and the kinematic viscosity at 40°C is 32.0-77.0 mm 2 / s.

[0011] As a preferred solution of the present invention: the polypropylene includes binary copolymer polypropylene and / or ternary copolymer polypropylene.

[0012] As a preferred embodiment of the present invention: the filler is at least one of silicon dioxide, talc, calcium carbonate, wollastonite and kaolin, and the average particle size of the filler is ≥2500 mesh.

[0013] As a preferred embodiment of the present invention: the hydrophilic modifier is selected from any one of polyethylene glycol, amino polyoxyethylene ether, polyoxyethylene oleyl ether, polyoxyethylene lauryl ether and methyl allyl polyoxyethylene ether, or a mixture of several of them.

[0014] As a preferred embodiment of the present invention: the antioxidant is selected from at least one of antioxidants 1076, 1010 and 168, or a mixture of two of them.

[0015] As a preferred embodiment of the present invention: the dispersant is one of ethylene bisstearamide, stearate, silane coupling agent and erucamide.

[0016] As a preferred embodiment of the present invention: a method for preparing a protein adsorption resistant TPE material specifically comprises the following steps:

[0017] S1. Weigh a certain amount of each component according to the ratio, mix SEBS with mineral oil, and fully absorb the oil;

[0018] S2, adding the remaining raw materials and stirring evenly to obtain a mixed material;

[0019] S3, adding the mixed material into a twin-screw extruder, and sequentially performing melt mixing, extrusion, cooling and granulation to obtain a protein adsorption resistant TPE material.

[0020] As a preferred solution of the present invention: the mixing and oil filling time of SEBS and mineral oil in S1 is 10-60 minutes, and the material extrusion temperature of the twin-screw extruder in S3 is 160-220°C.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The ethylene-butene segment in SEBS is compatible with PP, and PP has good impact resistance and fluidity, which can reduce the melt viscosity of SEBS to a certain extent, thereby improving its processing performance; in addition, the addition of PP can increase the physical cross-linking points of the composite system to improve the mechanical properties of SEBS and enhance the material's resistance to permanent deformation and creep. Different application requirements can be met by adjusting the ratio between the basic raw materials and process parameters; by adding hydrophilic additives, the material can be given better anti-protein adsorption properties. All materials used are safe and environmentally friendly raw materials, and have great application prospects in the field of direct or indirect contact with the human body. DETAILED DESCRIPTION

[0023] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] In view of the above problems, the purpose of the present invention is to provide a method for modifying a TPE material with resistance to protein adsorption and preparing the same, so as to prepare a TPE material with resistance to protein adsorption using low-cost raw materials. The present invention provides the following technical solutions:

[0025] Furthermore, SEBS is a linear block copolymer with an ethylene-butene copolymer obtained by hydrogenating polybutadiene as a middle elastic block.

[0026] Furthermore, the mineral oil is a paraffin-based white oil with a flash point of ≥200°C and a kinematic viscosity of 63.0-77.0 mm at 40°C. 2 / s.

[0027] Furthermore, the polypropylene includes terpolymer polypropylene.

[0028] Furthermore, the filler includes calcium carbonate, and the average particle size is ≥2500 mesh.

[0029] Furthermore, the hydrophilic modifier is amino polyoxyethylene ether.

[0030] Furthermore, the antioxidant is selected from at least one of antioxidants 1010 and 168 or a mixture of two of them.

[0031] Furthermore, a method for preparing a protein adsorption resistant TPE material specifically comprises the following steps:

[0032] S1. Weigh a certain amount of each component according to the ratio, mix SEBS with mineral oil, and fully absorb the oil;

[0033] S2, adding the remaining raw materials and stirring evenly to obtain a mixed material;

[0034] S3, adding the mixed material into a twin-screw extruder, and sequentially performing melt mixing, extrusion, cooling and granulation to obtain a protein adsorption resistant TPE material.

[0035] As a preferred solution of the present invention: the mixing and oil filling time of SEBS and mineral oil in S1 is 10-60 minutes, and the material extrusion temperature of the twin-screw extruder in S3 is 160-220°C.

[0036] Specifically, when used, the material proposed by the present invention is made of the following components in parts by weight:

[0037] Example 1

[0038] SEBS 25 parts

[0039] Mineral oil 50 parts

[0040] Polypropylene 20 parts

[0041] 5 parts filler

[0042] 2 parts of hydrophilic additive

[0043] Antioxidant 0.1 part

[0044] 0.3 parts of dispersant;

[0045] A method for producing a protein adsorption resistant TPE comprises the following steps:

[0046] Weigh a certain amount of each component according to the ratio, mix SEBS and mineral oil evenly, the oil filling time is 10-60min, add the remaining raw materials and stir evenly to obtain a mixed material. The above materials are melt-mixed, extruded, cooled and granulated through a twin-screw extruder at an extrusion temperature of 160-220°C to obtain a protein adsorption-resistant TPE material.

[0047] Example 2

[0048] SEBS 25 parts

[0049] 38 parts mineral oil

[0050] Polypropylene 23 parts

[0051] 5 parts of filler

[0052] 2 parts of hydrophilic additive

[0053] Antioxidant 0.1 part

[0054] 0.5 parts of dispersant;

[0055] A method for producing a protein adsorption resistant TPE comprises the following steps:

[0056] Weigh a certain amount of each component according to the ratio, mix SEBS and mineral oil evenly, the oil filling time is 10-60min, add the remaining raw materials and stir evenly to obtain a mixed material. The above materials are melt-mixed, extruded, cooled and granulated through a twin-screw extruder at an extrusion temperature of 160-220°C to obtain a protein adsorption-resistant TPE material.

[0057] Example 3

[0058] SEBS 41 parts

[0059] 41 parts of mineral oil

[0060] Polypropylene 13 parts

[0061] 5 parts of filler

[0062] 1 part hydrophilic additive

[0063] Antioxidant 0.1 part

[0064] 0.8 parts of dispersant;

[0065] A method for producing a protein adsorption resistant TPE comprises the following steps:

[0066] Weigh a certain amount of each component according to the ratio, mix SEBS and mineral oil evenly, the oil filling time is 10-60min, add the remaining raw materials and stir evenly to obtain a mixed material. The above materials are melt-mixed, extruded, cooled and granulated through a twin-screw extruder at an extrusion temperature of 160-220°C to obtain a protein adsorption-resistant TPE material.

[0067] Comparative Example 1

[0068] SEBS 41 parts

[0069] 41 parts of mineral oil

[0070] Polypropylene 13 parts

[0071] 5 parts of filler

[0072] Antioxidant 0.1 part

[0073] 0.8 parts of dispersant;

[0074] A method for producing a protein adsorption resistant TPE comprises the following steps:

[0075] Weigh a certain amount of each component according to the ratio, mix SEBS and mineral oil evenly, the oil filling time is 10-60min, add the remaining raw materials and stir evenly to obtain a mixed material. The above materials are melt-mixed, extruded, cooled and granulated through a twin-screw extruder at an extrusion temperature of 160-220°C to obtain a protein adsorption-resistant TPE material.

[0076] The materials prepared in the above Examples 1-3 and Comparative Example 1 were subjected to the following material performance tests, and the test results are as follows:

[0077]

[0078] Note: From the above test results, it can be seen that the anti-protein adsorption TPE material prepared in Examples 1-3 has good softness. The addition of hydrophilic additives improves the hydrophilicity of the TPE material without affecting the softness and mechanical properties of the material. The TPE material is superior to the silicone plugs on the market in terms of hydrophilicity (i.e., anti-protein adsorption performance) and sealing barrier performance.

[0079] Comparative Example 1 is a common TPE material that has not been hydrophilically modified. Its barrier property is still better than that of the silicone plug material, but its anti-protein adsorption performance is worse than that of Examples 1-3.

[0080] It can be seen from the above properties that the TPE material of the present invention has good mechanical properties, sealing barrier properties and anti-protein adsorption properties.

[0081] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A protein adsorption resistant TPE material, characterized in that: The components include, by weight, 10-40 parts of SEBS, 30-50 parts of mineral oil, 10-40 parts of polypropylene, 5-20 parts of filler, 1-5 parts of hydrophilic additive, 0.1-1 parts of antioxidant and 0.1-1 parts of dispersant.

2. The protein adsorption resistant TPE material according to claim 1, characterized in that: The SEBS is a linear block copolymer with an ethylene-butene copolymer obtained by hydrogenating polybutadiene as a middle elastic block, and the SEBS includes high-molecular SEBS and / or low-molecular SEBS.

3. The protein adsorption resistant TPE material according to claim 1, characterized in that: The mineral oil is paraffin-based mineral oil or naphthenic mineral oil. The flash point of the mineral oil is ≥200°C, and the kinematic viscosity at 40°C is 32.0-77.0 mm 2 / s.

4. The protein adsorption resistant TPE material according to claim 1, characterized in that: The polypropylene includes binary copolymer polypropylene and / or ternary copolymer polypropylene.

5. The protein adsorption resistant TPE material according to claim 1, characterized in that: The filler is at least one of silicon dioxide, talc, calcium carbonate, wollastonite and kaolin, and the average particle size of the filler is ≥2000 meshes.

6. The protein adsorption resistant TPE material according to claim 1, characterized in that: The hydrophilic modifier is selected from any one of polyethylene glycol, amino polyoxyethylene ether, polyoxyethylene oleyl ether, polyoxyethylene lauryl ether and methyl allyl polyoxyethylene ether, or a mixture of several of them.

7. The protein adsorption resistant TPE material according to claim 1, characterized in that: The antioxidant is selected from at least one of antioxidants 1076, 1010 and 168, or a mixture of two of them.

8. The protein adsorption resistant TPE material according to claim 1, characterized in that: The dispersant is one of ethylene bis stearamide, stearate, silane coupling agent and erucamide.

9. The method for preparing a protein adsorption resistant TPE material according to claims 1-8, characterized in that: The specific steps include: S1. Weigh a certain amount of each component according to the ratio, mix SEBS with mineral oil, and fully absorb the oil; S2, adding the remaining raw materials and stirring evenly to obtain a mixed material; S3, adding the mixed material into a twin-screw extruder, and sequentially performing melt mixing, extrusion, cooling and granulation to obtain a protein adsorption resistant TPE material.

10. The protein adsorption resistant TPE material according to claim 8, characterized in that: The mixing and oil filling time of SEBS and mineral oil in S1 is 10-60 minutes, and the material extrusion temperature of the twin-screw extruder in S3 is 160-220°C.