Low-silver mixed graphene ink, printing type radio frequency identification tag and preparation method of printing type radio frequency identification tag
By developing a method for preparing low-silver mixed graphene ink, the problems of high cost, severe pollution, and insufficient flexibility of printed RFID tags have been solved, resulting in reduced costs, improved conductivity, and expanded applications.
Patent Information
- Application Number
- CN202411535604.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-31
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing printed RFID tags are expensive, pollute the production process, and lack flexibility, while graphene RFID tags have insufficient conductivity, which limits their application.
Low-silver mixed graphene ink is formed by mixing silver paste and paste graphene ink in a specific ratio and then modifying it, and is used for the preparation of printable radio frequency identification tags.
It reduces label costs by approximately 50%, improves conductivity and flexibility, has a reading distance comparable to pure silver paste labels, and possesses stronger tensile and bending resistance.
Smart Images

Figure CN119039830A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of radio frequency identification tags, and in particular, relates to a low-silver mixed graphene ink, a printed radio frequency identification tag and a preparation method thereof. Background Art
[0002] As the "identity card" of commodities, UHF-RFID tags are the window for commodity information to interact with the Internet of Things. At present, UHF-RFID tags are mainly realized by acid-etching metal films, which have defects such as cumbersome processes, serious environmental pollution, poor mechanical toughness of products, and the need to use acid-resistant substrates. Printed radio frequency tags print conductive paste directly onto packaging to form a tag antenna structure. The processing steps are simple and pollution-free. It can be applied to different substrates and has obvious advantages over traditional processes.
[0003] At present, mature printed RFID is mainly printed by conductive silver paste, such as Chinese patent "CN101921505B A conductive ink composition for printing wireless radio frequency identification system", Chinese patent "CN103275559B A conductive ink for RFID printing and its preparation method", etc., which describe the preparation method of conductive paste for RFID with silver as the conductive phase. In recent years, people have tried to use low-dimensional carbon materials to replace silver powder, such as Chinese patent "CN117735536A A graphene RFID tag and its preparation method and application", "CN113773698A A graphene RFID electronic tag and its preparation method", SCI journal nature communication document (DOI: 10.1038 / s41467-018-07632-w), etc., which describe the preparation method of radio frequency identification tags based on graphene paste.
[0004] Currently, printed RFID tags mainly use low-temperature silver paste because this type of material has high conductivity and stable performance. However, due to cost constraints, this type of tag is generally expensive and is only suitable for a few high value-added industries. Low-dimensional carbon materials, such as graphene and carbon nanotube pastes, are believed to have the potential to replace low-temperature silver pastes. However, the conductivity of such pastes is generally around 10 3 -10 4 S / m is much lower than that of silver paste, so the printed antenna based on this type of paste needs to make compromises in structure, size, thickness, etc. Other pastes, such as liquid metal and two-dimensional inorganic compounds, are still in the feasibility verification stage due to cost, technology and stability issues, and cannot be industrialized in a short time. Summary of the invention
[0005] The purpose of the present application is to provide a low-silver mixed graphene ink, a printed radio frequency identification tag and a preparation method thereof to at least solve one of the problems in the prior art, such as high cost, pollution in production, insufficient flexibility, and poor performance of graphene-doped RFID tags.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions: In a first aspect, a low-silver mixed graphene ink for printed radio frequency identification tags is provided, wherein the slurry composition is as follows by weight: 2 parts of silver paste and 3-8 parts of pasty graphene ink; wherein: The paste-like graphene ink comprises 6-12 wt % of graphene micro / nano sheets, 0.6-1 wt % of cellulose acetate butyrate, and the remainder is an organic solvent; The silver paste is composed of a silver micro-flake organic carrier and silver micro-flakes in a mass ratio of 1:3.
[0007] In the above-mentioned low silver content graphene ink, as a preferred embodiment, the size of the silver micro-sheets is 0.5-1 μm, and the size of the graphene micro / nano-sheets is 0.5-1.2 μm.
[0008] In the above-mentioned low silver content mixed graphene ink, as a preferred embodiment, in the paste-like graphene ink, the organic solvent is selected from at least one of dihydro-levulinic ketone, n-methyl pyrrolidone and dimethylformamide.
[0009] In the above-mentioned low-silver mixed graphene ink, as a preferred embodiment, the organic solvent is dihydro-levulinic ketone, and in the slurry composition, the content of dihydro-levulinic ketone ranges from 50-72%, the content of the silver microsheets is 15-20%; and the content of the graphene micro / nanosheets is 6-8%.
[0010] In the above-mentioned low-silver mixed graphene ink, as a preferred embodiment, the composition of the silver micro-sheet organic carrier is polyurethane resin, diethylene glycol butyl ether, hexamethyl anhydride curing agent and 3-(trimethoxymethylsilyl)propyl methacrylate in a mass ratio of 1:1:0.5:0.1.
[0011] In the above-mentioned low-silver mixed graphene ink, as a preferred embodiment, the silver paste is further added with the silver microsheet organic carrier and the silver microsheet mass and 0.8-1.2% of cysteamine.
[0012] In a second aspect, a method for preparing a low silver mixed graphene ink is provided, comprising the following steps: S1, preparation of a paste-like graphene ink: dissolving dried graphene micro / nano sheets in dihydro-L-glucose ketone, adding cellulose acetate butyrate, and stirring to form a paste-like graphene ink; in the paste-like graphene ink, the content of the graphene micro / nano sheets is 6-12wt%, and the content of the cellulose acetate butyrate is 0.6-1wt%; S2, preparation of silver paste: firstly, polyurethane resin, diethylene glycol butyl ether, methyl hexachloride curing agent and 3-(trimethoxymethylsilyl) propyl methacrylate are mixed in a weight ratio of 1:1:0.5:0.1, and stirred to form a silver micro-sheet organic carrier; the silver micro-sheet organic carrier and the silver micro-sheets are mixed and stirred to form a coarse silver paste, wherein the weight ratio of the organic carrier to the silver micro-sheets in the coarse silver paste is 1:3; the coarse silver paste is subjected to roller grinding and filtering to form a silver paste; S3, preparation of low silver mixed graphene ink: mixing the silver paste obtained in step S2 and the paste-like graphene ink obtained in step S1 in a weight ratio of 2:3-8, stirring, and standing in a vacuum oven at room temperature to form the low silver mixed graphene ink.
[0013] In the preparation method of the low-silver mixed graphene ink mentioned above, as a preferred embodiment, a silver paste modification step is also included before step S3, and cysteamine is added to the silver paste obtained in step S2 for modification. The amount of cysteamine added is 0.8-1.2% of the sum of the mass of the silver microsheet organic carrier and the silver microsheet.
[0014] In the above-mentioned method for preparing low-silver mixed graphene ink, as a preferred embodiment, in step S1, the method for preparing graphene micro / nano sheets comprises the following steps: S11, placing 75 mesh expandable organic intercalated graphite in a microwave oven at 800W for 30s to achieve graphite expansion; S12, the expanded graphite is dissolved in dihydro-L-glucose ketone at a concentration of 10 mg / ml, and the mixed solution is placed in a 180W, 40kHz ultrasonic pool for 15 hours to perform graphene micro / nanosheet exfoliation. During the exfoliation process, ice cubes are continuously added to the ultrasonic pool to prevent graphite oxidation; S13, the graphene solution after stripping is centrifuged at 300 rpm for 10 minutes, the supernatant is taken, and passed through a 300-mesh steel sieve, and the process is repeated 3 times to remove large particles that have not been stripped, thereby forming a graphene dispersion; S14, the dispersion is centrifuged at 2000 rpm, the graphene sediment is taken out, and dried to obtain the graphene micro / nano sheets.
[0015] In the above-mentioned method for preparing low-silver mixed graphene ink, as a preferred embodiment, the size of the silver micro-sheets is 0.5-1 μm, and the size of the graphene micro / nano-sheets is 0.5-1.2 μm.
[0016] In the above-mentioned method for preparing low-silver mixed graphene ink, as a preferred embodiment, in step S2, stirring at 1000 rpm for 1 hour to form the silver micro-sheet organic carrier; when mixing the silver micro-sheet organic carrier and the silver micro-sheet, the silver micro-sheet is added in batches; the crude silver paste is subjected to a three-roll mill grinding treatment for 3 times, and passed through a 300-mesh filter to form the silver paste; In step S3, the silver paste and the pasty graphene ink are stirred at 500 rpm for 1 hour, and then left to stand at room temperature in a vacuum oven for 3 hours to form the low silver mixed graphene ink.
[0017] In the preparation method of the above-mentioned low-silver mixed graphene ink, as a preferred embodiment, in step S2, the batch addition is: first mix the organic carrier and the silver microflakes in a 1:1 ratio by weight, add an equal amount of silver microflakes after stirring at 3000rpm for 30 minutes, then add the same amount of silver microflakes again after stirring for another 30 minutes, and continue stirring for 2 hours to form a coarse silver paste, at which time the ratio of silver microflakes to organic carrier in the coarse silver paste is 75:25.
[0018] In a third aspect, a printed radio frequency identification tag of low silver mixed graphene is provided, which is prepared using the above-mentioned low silver mixed graphene ink.
[0019] In a fourth aspect, a method for preparing the printed radio frequency identification tag of the low silver mixed graphene is provided, comprising: First, the antenna structure was printed onto the substrate using a 200 mesh screen printer. o C drying for 30 minutes; Secondly, the antenna structure is placed at 165 o C. Metal roller pressing twice under 6MPa; Then, glue is dispensed using a glue dispenser, and the chip is welded in the center of the antenna using a packaging machine. o C. After 15 seconds of hot pressing, the RFID tag is formed; The substrate is selected from any one of TPU, coated paper, non-woven fabric, glass, and PET.
[0020] Compared with the prior art, the solution of this application has the following beneficial effects: 1) Aluminum foil etching is the mainstream technology for the preparation of radio frequency tags. Compared with aluminum foil etching, the tag in this application has the same performance and reduces the cost by 20%. It also has the advantages of pollution-free production, flexibility, and no risk of falling off; 2) Pure silver will be widely reported as a paste for printed RFID applications, but due to its high cost, it is difficult to achieve industrial application. The maximum reading distance of the label in this application is 9 meters, which is equivalent to that of pure silver paste printed labels, but the silver content of the paste is only 1 / 5 of that of pure silver paste, the label cost is about 50% lower, and it has stronger tensile and bending resistance.
[0021] 3) Although there are reports of RFID tags based on graphene and carbon nanotubes, due to the insufficient conductivity of graphene (10 3 -10 4 S / m), so it can only be used to design thick and large-sized tags, and the reading distance is small, and the application is highly limited. This project adds a small amount of silver to make the slurry conductivity reach 3.7 × 10 5 , which is more than 10 times that of pure carbon materials. It can be used in small and medium-sized label designs, and the reading distance is close to that of pure silver labels. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The Raman images of graphene at different peeling times in Example 1, where (a) is the overall spectrum and (b) is the 2D regional spectrum; Figure 2 This is the SEM image of the graphene ink print in Example 1; Figure 3 This is a structural diagram of a printed label in Example 1; Figure 4 This is the SEM image of the printed product with 15% silver micro-flakes added with graphene ink in Example 1; Figure 5 The comparison diagram of the printed labels obtained in Comparative Example 1, Comparative Example 4 and Example 1 after being rubbed 10 times, wherein (a), (b) and (c) are pictures of the printed labels obtained in Comparative Example 1, Comparative Example 4 and Example 1 after being rubbed 10 times respectively; Figure 6 This is the relationship curve between square resistance (after roller pressing) and silver content; Figure 7 The following is a comparison chart of reading distances of different embodiments. DETAILED DESCRIPTION
[0023] The present application provides a low silver mixed graphene ink for printed radio frequency identification tags, labels and preferred embodiments of the preparation method thereof as follows: A low-silver mixed graphene ink for printed radio frequency identification tags, wherein the slurry composition is as follows by weight: 2 parts of silver paste and 3-8 parts of pasty graphene ink; wherein: The paste-like graphene ink comprises 6-12 wt % of graphene micro / nano sheets, 0.6-1 wt % of cellulose acetate butyrate, and the remainder is an organic solvent; The silver paste is composed of a silver micro-flake organic carrier and silver micro-flakes in a mass ratio of 1:3.
[0024] In the above slurry composition, silver microsheets and graphene micro / nanosheets are conductive phases of the slurry for electron transmission. Preferably, the size of the silver microsheets is 0.5-1 μm (such as 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, etc.), and the size of the graphene micro / nanosheets is 0.5-1.2 μm (such as 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1.0 μm, 1.1 μm, etc.). If the size of the silver microsheets and graphene micro / nanosheets is too large or too small, the dispersion uniformity of the silver microsheets and graphene will be reduced. The dispersion effect is best when the size of the silver microsheets and graphene is close.
[0025] In the above slurry composition, the content of silver micro-sheets is about 15-30% (such as 18%, 20%, 25%, 28%, 17%, etc.), and the preferred content is about 15-20% (such as 16%, 17%, 18%, 19%, etc.). If the silver content is lower than this range, such as as low as about 5% or 10%, it is easy to cause insufficient performance. If it is higher than this range, such as about 40%, 50% or 60%, the cost will increase, and the performance will not be greatly improved. The inventors have found through experiments that a small increase in the proportion of silver micro-sheets (below 50%) has almost no improvement in the conductivity of the slurry, but will increase the cost of the slurry. The silver content is increased from the above suitable range to 50%, but the conductivity is slightly improved, and the cost will increase significantly.
[0026] The above-mentioned paste-like graphene ink component includes 6-12wt% of graphene micro / nano sheets, 0.6-1wt% of cellulose acetate butyrate, and the balance is an organic solvent.
[0027] In the above slurry composition, the content of graphene micro / nano sheets is about 6-10% (such as 6.5%, 7%, 8%, 9%, etc.). If the content is too high, the slurry cannot be effectively dispersed, and if it is too low, it will affect the conductivity of the graphene film after forming; the preferred content is about 6-8% (such as 6.5%, 7%, 7.5%, etc.). If the proportion of graphene is further increased, the conductivity of the slurry will be reduced.
[0028] In the above-mentioned low-silver mixed graphene ink, as a preferred embodiment, in the paste-like graphene ink, the organic solvent is selected from at least one of dihydro-levulinic ketone, n-methylpyrrolidone and dimethylformamide; more preferably dihydro-levulinic ketone.
[0029] As a carrier of graphene, dihydro-levulinic ketone usually increases the thickness of graphene and reduces the conductivity of graphene by secondary stacking. However, the Hansen solubility parameter of dihydro-levulinic ketone is close to that of graphene, so graphene will not be secondary stacked in this carrier, which can prevent the (few layers) graphene in the slurry from secondary stacking due to the π-π effect, thereby reducing the conductivity of graphite. The content of dihydro-levulinic ketone in the above-mentioned slurry composition of the present invention is in the range of about 50-72% (such as 52%, 55%, 60%, 65%, 68%, 70%, etc.). If the content is too much or too little, it will affect the viscosity and dispersibility of the slurry. The dihydro-levulinic ketone can be replaced by any one of n-methylpyrrolidone and dimethylformamide.
[0030] The main function of cellulose acetate butyrate is to improve the adhesion of the slurry. The cellulose acetate butyrate content in the above slurry composition of the present invention is about 0.6-1% (such as 0.7%, 0.8%, 0.9%, etc.). Too much will reduce the conductivity of the slurry, and too little will lead to insufficient adhesion of the slurry.
[0031] In the above-mentioned low-silver mixed graphene ink, as a preferred embodiment, the silver paste is further added with the silver microsheet organic carrier and the silver microsheet mass and 0.8-1.2% of cysteamine.
[0032] Cysteamine is used to modify the silver microsheets, and its addition amount is 0.8-1.2% of the total mass of the silver microsheet organic carrier and the silver microsheet, preferably 1%. Too low an addition amount will affect the dispersion efficiency of the silver microsheets and graphene, and too high an addition amount will affect the conductivity of the slurry.
[0033] As a preferred embodiment of the low-silver mixed graphene ink, the silver micro-sheet organic carrier is composed of a polyurethane resin, diethylene glycol butyl ether, methyl hexachloride curing agent and 3-(trimethoxymethylsilyl)propyl methacrylate in a mass ratio of 1:1:0.5:0.1.
[0034] Polyurethane resin is the resin carrier and diethylene glycol butyl ether is the resin solvent, which are mixed to form a silver micro-sheet carrier. Too much carrier will reduce the conductivity of the slurry, and too little carrier will cause uneven dispersion of the silver paste.
[0035] Formic anhydride curing agent is a low-temperature curing agent used to achieve low-temperature curing of the slurry. Too much will affect the conductivity of the slurry, and too little will make the slurry difficult to cure.
[0036] 3-(Trimethoxymethylsilyl) propyl methacrylate is an auxiliary coupling agent, and too much or too little will affect the rheological properties of the slurry. The 3-(trimethoxymethylsilyl) propyl methacrylate can be replaced by turpentine.
[0037] A method for preparing low-silver mixed graphene ink comprises the following steps: S1, preparation of a paste-like graphene ink: dissolving dried graphene micro / nano sheets in dihydro-L-glucose ketone, adding cellulose acetate butyrate, and stirring to form a paste-like graphene ink; in the paste-like graphene ink, the content of the graphene micro / nano sheets is 6-12wt%, and the content of the cellulose acetate butyrate is 0.6-1wt%; S2, preparation of silver paste: firstly, polyurethane resin, diethylene glycol butyl ether, methyl hexachloride curing agent and 3-(trimethoxymethylsilyl) propyl methacrylate are mixed in a weight ratio of 1:1:0.5:0.1, and stirred to form a silver micro-sheet organic carrier; the silver micro-sheet organic carrier and the silver micro-sheets are mixed and stirred to form a coarse silver paste, wherein the weight ratio of the organic carrier to the silver micro-sheets in the coarse silver paste is 1:3; the coarse silver paste is subjected to roller grinding and filtering to form a silver paste; S3, preparation of low silver mixed graphene ink: mixing the silver paste obtained in step S2 and the paste-like graphene ink obtained in step S1 in a weight ratio of 2:3-8, stirring, and standing in a vacuum oven at room temperature to form the low silver mixed graphene ink.
[0038] In the above-mentioned method for preparing low-silver mixed graphene ink, as a preferred embodiment, a silver paste modification step is also included before step S3, and cysteamine is added to the silver paste obtained in step S2 for modification. The amount of cysteamine added is 0.8-1.2% of the sum of the mass of the silver microsheet organic carrier and the silver microsheet, and the preferred amount added is 1%.
[0039] In the above-mentioned method for preparing low-silver mixed graphene ink, as a preferred embodiment, in step S1, the method for preparing graphene micro / nano sheets comprises the following steps: S11, placing 75 mesh expandable organic intercalated graphite in a microwave oven at 800W for 30s to achieve graphite expansion and reduce the interlayer π-π interaction of graphite. After microwave treatment, the volume of graphite expands by 2-3 times (observed with naked eyes); S12, the expanded graphite is dissolved in dihydro-L-glucose ketone at a concentration of 10 mg / ml, and the mixed solution is placed in a 180W, 40kHz ultrasonic pool for 15 hours to perform graphene micro / nanosheet exfoliation. During the exfoliation process, ice cubes are continuously added to the ultrasonic pool to prevent graphite oxidation; S13, the graphene solution after stripping is centrifuged at 300 rpm for 10 minutes, the supernatant is taken, and passed through a 300-mesh steel sieve, and the process is repeated 3 times to remove large particles that have not been stripped, thereby forming a graphene dispersion. The dispersion is left standing in the air for 24 hours without obvious precipitation (observed with the naked eye); S14, the dispersion was centrifuged at 2000 rpm, the graphene sediment was taken out, and the graphene micro / nano sheets were obtained after drying. The weighing results showed that according to the above method, about 40% of the graphite was successfully exfoliated, and the Raman results showed that there were no defects in the exfoliation process and the thickness was a few layers (see Figure 1 ). The advantage of this preparation method is that the size uniformity of the obtained graphene micro / nano sheets is better, which is more conducive to ensuring the subsequent dispersion effect.
[0040] In the preparation method of the above-mentioned low-silver mixed graphene ink, as a preferred embodiment, the size of the silver microflakes is 0.5-1μm (for example, 0.6μm, 0.7μm, 0.8μm, 0.9μm, etc.), and the size of the graphene micro / nano flakes is 0.5-1.2μm (for example, 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1.0μm, 1.1μm, etc.).
[0041] In the above method for preparing low-silver mixed graphene ink, as a preferred embodiment, in step S2, stirring is performed at 1000 rpm for 1 hour to form the silver micro-sheet organic carrier.
[0042] In the preparation method of the low-silver mixed graphene ink mentioned above, as a preferred embodiment, in step S2, when mixing the silver microflakes organic carrier and the silver microflakes, the silver microflakes are added in batches; more preferably, the organic carrier and the silver microflakes are first mixed in a 1:1 ratio by weight, and then an equal amount of silver microflakes are added after stirring at 3000 rpm for 30 minutes, and then an equal amount of silver microflakes are added again after stirring for another 30 minutes, and stirring is continued for 2 hours to form a coarse silver paste, at which time the ratio of silver microflakes to organic carrier in the coarse silver paste is 75:25.
[0043] In the above-mentioned method for preparing low-silver mixed graphene ink, as a preferred embodiment, in step S2, the crude silver paste is subjected to a three-roll mill grinding treatment for 3 times and passed through a 300-mesh filter to form the silver paste.
[0044] In the above method for preparing low-silver mixed graphene ink, as an alternative implementation, in step S2, the 3-(trimethoxysilyl)propyl methacrylate can be replaced by turpentine.
[0045] In the above-mentioned method for preparing low-silver mixed graphene ink, as a preferred embodiment, in step S3, the silver paste and the paste graphene ink are stirred at 500 rpm for 1 hour, and then left to stand at room temperature in a vacuum oven for 3 hours to form the low-silver mixed graphene ink.
[0046] A low-silver mixed graphene printed radio frequency identification tag is prepared by using the low-silver mixed graphene ink.
[0047] A method for preparing the above-mentioned printed radio frequency identification tag of low silver mixed graphene comprises: First, the antenna structure was printed onto the substrate using a 200 mesh screen printer. o C drying for 30 minutes; Secondly, the antenna structure is placed at 165 o C. Metal roller pressing twice under 6MPa; Then, glue is dispensed using a glue dispenser, and the chip is welded in the center of the antenna using a packaging machine. o C. The RFID tag is formed after 15 seconds of heat pressing.
[0048] Preferably, the substrate is selected from any one of TPU, coated paper, non-woven fabric, glass, PET and the like.
[0049] The present invention will be further described in detail below through examples. The protection scope of the present invention includes but is not limited to the following examples.
[0050] If no specific experimental steps or conditions are specified in the examples, the experiments can be carried out according to the conventional steps or conditions described in the literature in the art.
[0051] Unless otherwise specified, all reagents and raw materials used in the examples are commercially available products.
[0052] Example 1 The method for preparing the printed RFID tag of low silver mixed graphene of this embodiment comprises the following steps: Step 1. Place 75 mesh expandable organic intercalated graphite in a microwave oven at 800W for 30s to expand the graphite and reduce the interlayer π-π interaction of the graphite. After microwave treatment, the volume of the graphite expands by 2-3 times (observed with the naked eye).
[0053] Step 2. The expanded graphite was dissolved in dihydro-L-glucose ketone at a concentration of 10 mg / ml. The mixed solution was placed in a 180W, 40kHz ultrasonic pool for 15 hours to exfoliate the graphene micro / nano sheets. Ice cubes were continuously added to the ultrasonic pool during the exfoliation process to prevent graphite oxidation.
[0054] Step 3. After exfoliation, the graphene solution was centrifuged at 300 rpm for 10 minutes, and the supernatant was taken and passed through a 300-mesh steel sieve. This process was repeated three times to remove the unexfoliated large particles and form a graphene dispersion. The dispersion was left in the air for 24 hours without any obvious precipitation (observed by naked eye).
[0055] Step 4. The dispersion was centrifuged at 2000 rpm and the graphene sediment was taken. After drying, the weight results showed that according to the above method, about 40% of the graphite was successfully exfoliated. Raman results showed that there were no defects in the exfoliation process and the thickness was a few layers (see Figure 1 ). Figure 1 The Raman images of graphene at different peeling times (0 hours, 5 hours, 10 hours, and 15 hours) are shown in Figure 2. Figure 1 As can be seen from (a) in the figure, no D peak appears in all Raman images, proving that no defects are introduced during peeling. Figure 1As can be seen in (b), the 2D peak of unpeeled graphite is accompanied by a shoulder (0 hours), and the shoulder disappears after 15 hours of peeling, proving that the graphene after peeling is a few layers. Except for the graphene obtained by ultrasonic peeling for 15 hours in this example, the graphene with other peeling times is not used for labeling because its sheet resistance is extremely high (80-150 Ω / sq) and has no application value.
[0056] Step 5. Dissolve the dried graphene in dihydro-L-glucose ketone at 10 wt% (weight percentage), add 1 wt% (weight percentage) of cellulose acetate butyrate, and stir at 1000 rpm for 1 hour to form a paste-like graphene ink. After screen printing with 200 mesh, the ink has a 10-micron thick surface resistance of 29 Ω / sq (conductivity of 3.4×10 3 S / m), scanning electron microscopy shows that the size of the printed graphene sheets is 0.5-1.2 microns (see Figure 2 ).
[0057] Step 6. Mix polyurethane resin, diethylene glycol butyl ether, methyl hexachloride curing agent and 3-(trimethoxymethylsilyl)propyl methacrylate in a weight ratio of 1:1:0.5:0.1, and stir at 1000 rpm for 1 hour to form a silver microsheet organic carrier.
[0058] Step 7. Mix the organic carrier and silver microflakes (flake size 0.5-1 micron, Zhejiang Shengde flaky silver powder) in a 1:1 ratio, stir at 3000rpm for 30 minutes, add the same amount of silver microflakes, stir for another 30 minutes, add the same amount of silver micropowder again, and continue stirring for 2 hours to form a coarse silver paste (the ratio of silver microflakes to organic carrier in the coarse silver paste is 75:25).
[0059] Step 8. Grind the crude silver paste three times with a three-roll mill and filter it through a 300-mesh filter to form a silver paste (75% silver). After screen printing with 200 mesh, the silver paste has a 10-micron thick surface resistance of 80 mΩ / sq (conductivity of 1.25×10 6 S / m).
[0060] Step 9. Add 1% by weight of cysteamine to the silver paste to modify the silver microflakes, then mix with the paste graphene ink (prepared in step 5) in a weight ratio of 2:8, stir at 500 rpm for 1 hour, and let stand in a vacuum oven at room temperature for 3 hours to form a low-silver mixed graphene ink (silver content 15%).
[0061] Step 10. Use 200 mesh screen printing to print the antenna structure (see Figure 3 ) printed on coated paper substrate, 120 o C for 30 minutes. The antenna structure was dried at 165 o C, after metal roller pressing twice under 6MPa, the thickness is 6 microns, the surface resistance is 0.45 Ω / sq (conductivity is 3.7×105 S / m). See the SEM image of the printed antenna. Figure 4 . Use a dispensing machine (DELOMONOPOX AC268) to dispense glue, and use a packaging machine to solder a chip (NXP's UCODE 8 chip, reading sensitivity -23 dBm) in the center of the antenna, and heat press (140 o C15 seconds) to form an RFID tag. The E side of the tag is 0 o , when the transmission power is 33dBm, the maximum reading distance is 9m (see reading distance Figure 7 ).
[0062] The conductivity of the coated paper base label prepared in this embodiment reaches 3.7×10 5 S / m, compared with graphene labels (conductivity 10 3 -10 4 The maximum reading distance is 9m, which is equivalent to that of pure silver paste printed labels, but the silver content of the paste is only 1 / 5 of that of pure silver paste, and the label cost is reduced by about 50%; it has stronger tensile and bending resistance.
[0063] Comparative Example 1 This comparative example prepares a pure graphene printed label.
[0064] The pure graphene slurry in step 5 of Example 1 was placed in a vacuum oven at room temperature for 3 hours, and then taken out and step 10 of Example 1 was repeated.
[0065] Comparative Example 2 In this comparative example, a 50% high silver mixed graphene printed label was prepared.
[0066] The modified silver paste prepared in step 9 of Example 1 was mixed with the graphene ink prepared in step 5 of Example 1 in a weight ratio of 1:0.5, stirred at 500 rpm for 1 hour, and allowed to stand in a vacuum oven at room temperature for 3 hours to form a high-silver mixed graphene ink (silver content 50%), and step 10 in Example 1 was repeated.
[0067] Comparative Example 3 This comparative example prepares a 15% low silver (spherical) mixed graphene printed label.
[0068] The flake silver powder in step 7 of Example 1 was replaced with spherical silver powder (size 0.5-1 μm), and steps 8-10 of Example 1 were repeated.
[0069] Comparative Example 4 This comparative example prepares a pure silver paste printed label.
[0070] Prepare the pure silver paste in step 8 of Example 1, let it stand in a vacuum oven at room temperature for 3 hours, and repeat step 10 of Example 1.
[0071] Performance Testing 1. Slurry property test.
[0072] The test method is as follows: The antenna structure can be printed on coated paper by 200 mesh screen printing, 120 o C for 30 minutes and then dried at 165 o C, metal roller pressed twice under 6MPa conditions. The square resistance of the antenna print was tested using a four-probe square resistance meter (DWR1C, Shanghai Instruments). The four probes were placed on the diagonal of the antenna dipole and the corresponding square resistance values were read. The film thickness was measured using a film thickness meter, and the square resistance was converted into conductivity. The test results are shown in Table 1: Table 1 Slurry properties (printing substrate is coated paper)
[0073] It can be seen from Table 1 that although the cost of Comparative Example 1 is lower, its conductivity is nearly 30 times lower than that of the slurry in Example 1, and its use in printing RFID antennas will result in serious performance deficiencies. Compared with Comparative Example 2, Example 1 has lower silver content and cost, but almost the same performance, proving that when the silver content exceeds 15% and further increases (≤50%), the conductivity gain of the slurry is very small. Compared with Comparative Example 3, Example 1 has an advantage of more than 5 times in conductivity at the same cost, proving that the interface resistance transmission efficiency of flaky silver powder and graphene is higher than that of spherical silver powder. The conductivity of Comparative Example 4 is higher than that of Example 1 and Comparative Example 2, proving that when the silver content exceeds 50%, further increasing the silver content will continue to improve the conductivity of the slurry, but the cost will also increase sharply. For example, the cost of Comparative Example 4 is about 3 times that of Example 1, which greatly limits the application of antennas based on Comparative Example 4 in potential application scenarios.
[0074] 2. Test the adaptability to different substrates.
[0075] The test method is as follows: The low-silver mixed graphene ink prepared in Example 1 is used to print the antenna structure onto different substrates (coated paper, PET, TPU, glass, non-woven fabric, thermal transfer adhesive) by 200 mesh screen printing. o After drying at 80 o C, metal roller pressed twice under 6MPa (TPU and non-woven fabric 165 o C roller pressure will cause obvious deformation). The square resistance of the antenna print is tested using a four-probe square resistance meter (DWR1C, Shanghai Instruments). The four probes are placed on the diagonal of the antenna dipole and the corresponding square resistance value is read. This value is divided by the square resistance value of the antenna on the coated paper to obtain the change in conductivity of the slurry on different substrates. The test results are shown in Table 2.
[0076] Table 2 Test results of adaptability to different substrates
[0077] The data in the table are the ratios of conductivity to conductivity on coated paper, and the calculation formula is: (conductivity on the corresponding substrate) / (conductivity on coated paper).
[0078] It can be seen from Table 2 that all the slurries exhibit high conductivity on dense surfaces such as coated paper, PET, and glass, while the conductivity decreases on flexible substrates such as TPU (thermoplastic polyurethane elastomer, also known as thermoplastic polyurethane rubber), non-woven fabrics, and thermal transfer adhesives. Among them, the conductivity attenuation of Example 1, Comparative Example 1 and Comparative Example 3 on flexible substrates is much smaller than that of Comparative Example 2 and Comparative Example 4, mainly because the above three examples have a higher graphene content, and therefore have better material flexibility than silver sheets.
[0079] 3. Test on rubbing tensile stability (TPU substrate).
[0080] The test method is as follows: The antenna structure can be printed on TPU by 200 mesh screen printing, 120 o After drying at 80 o C, metal roller pressed twice under 6MPa. The square resistance of the antenna printed product was tested by a four-probe square resistance meter (DWR1C, Shanghai Instruments), the film thickness was measured by a film thickness meter, and the square resistance was converted into conductivity.
[0081] During the stretching test, two metal clips are used to clamp the two ends of the TPU and stretch them to 105% of the original length. The conductivity of the antenna is measured in the same way and compared with that before stretching to determine the tensile strength of the antenna. During the rubbing test, the antenna is folded along the central axis, the dipoles at both ends are in contact and rubbed vigorously for 10 times, then opened, the conductivity of the antenna is measured and compared with that before rubbing to determine the stability of the antenna under extrusion and rubbing. Figure 5 The following are comparison diagrams of the printed labels obtained in Comparative Example 1, Comparative Example 4 and Example 1 after being rubbed 10 times respectively, wherein (a), (b) and (c) are pictures of the printed labels obtained in Comparative Example 1, Comparative Example 4 and Example 1 after being rubbed 10 times respectively.
[0082] The results of the rubbing tensile stability test are shown in Table 3 below.
[0083] Table 3 Rub and stretch stability test (TPU substrate)
[0084] As can be seen from Table 3, the square resistance of the pure silver paste (Comparative Example 4) will increase significantly after stretching and rubbing, indicating that its stretching and extrusion resistance are obviously insufficient. The pure graphene paste (Comparative Example 1) has excellent stretch resistance, but some graphene will fall off after strong friction, resulting in a decrease in conductivity. The embodiment and comparative examples 2 and 3 show excellent friction resistance and stretch resistance, proving that they are suitable for scenes such as clothing and wearable devices.
[0085] 4. Reading distance test The test method is as follows: the forward and reverse power of the tag is tested by Voyantic's Tagformance Pro RFID system, and converted into forward and reverse reading distances, and the minimum value between the two is taken. Since the tag reading distance depends not only on the antenna conductivity but also on the antenna-chip impedance matching, the direct comparison of the reading distance between Example 1 and the comparative example lacks practical significance. The reading distance of the tag prepared in Example 1 is 9 meters (spectrum 915MHz, E plane is 0 o , Figure 7 ), which is comparable to known pure silver printed labels, thanks to the low silver content, the total cost of the label can be reduced by about 50%.
[0086] Example 2 The steps of this embodiment are the same as those of embodiment 1, except that no metal rolling treatment is performed when preparing the RFID tag in step 10, i.e., the step of "metal rolling the antenna structure twice at 165° C. and 6 MPa" in step 10 is not performed.
[0087] Example 3 The steps of this embodiment are the same as those of embodiment 1, except that in step 9, the unmodified silver microflakes are directly mixed with the graphene ink in a weight ratio of 2:8, stirred at 500 rpm for 1 hour, and allowed to stand in a vacuum oven at room temperature for 3 hours to form a low silver content graphene ink.
[0088] Example 4 The steps of this embodiment are the same as those of embodiment 1, except that step 9 is changed to: adding 1% by weight of cysteamine to the silver paste to modify the silver microsheets, and mixing with the paste graphene ink (prepared in step 5) according to the weight ratio in Table 4, stirring at 500 rpm for 1 hour, and standing in a vacuum oven at room temperature for 3 hours to form different silver-containing mixed graphene inks, as shown in Table 4: Table 4 Example 4 Mixtures of different weight proportions and corresponding silver content
[0089] Conductivity test: The square resistance of the antenna print was tested using a four-probe square resistance meter (DWR1C, Shanghai Instruments). The four probes were placed on the diagonal of the antenna dipole and the corresponding square resistance was read. The film thickness was measured using a film thickness meter, and the square resistance was converted into conductivity. The test results are shown in Table 5. The relationship curve between square resistance (after roller pressing) and silver content is shown in Figure 6 .
[0090] Table 5 Slurry properties (printing substrate is coated paper)
[0091] As can be seen from Table 5, Example 2 has the same silver content as Example 1, but the surface resistance is twice as high as that of Example 1, while the conductivity is 1 / 4 of that of Example 1 (because the thickness difference is about 1 times). This shows that after the roller is pressed, the conductivity of the printed product is improved due to the increase in the contact area between the graphene and the silver microsheets. The conductivity of Example 3 is about half of that of Example 1, which shows that the connection effect of the molecular bridge can effectively improve the interface transmission efficiency between the graphene and the silver microsheets. Examples 4.1-4.2 show that when the silver content is lower than that of Example 1, the conductivity of the printed product is much lower than that of Example 1, which will seriously affect the working efficiency as an antenna. In Examples 4.3-4.6, although the silver content is higher than that of Example 1, the conductivity has no obvious advantage over Example 1, and is only improved by ~10%-20%, but the cost is greatly increased. The conductivity of Example 4.7 is significantly improved compared with Example 1, but the cost is too high (about 2.5 times that of Example 1), which will significantly increase the cost of the tag as a tag antenna.
[0092] Examples 2-4 all show substrate suitability, bending resistance and stretch resistance similar to those of Example 1, but due to the limitation of conductivity, the printed antenna reading distance of Examples 2, 3, 4.1 and 4.2 is much lower than that of Example 1 under the same size, while the reading distance of Examples 4.3-4.7 is close to that of Example 1, but the cost is higher than that of Example 1 (see Figure 7 ). The reading distance test method is as follows: Use Voyantic's Tagformance Pro RFID system to test the tag's forward and reverse power, and convert it into forward and reverse reading distances, taking the minimum value between the two.
[0093] It should be noted that, in the present invention, except for the understanding otherwise in conjunction with the full text, if any, the relevant terms should be understood as follows. Relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. Moreover, the term "includes", "comprising" or any other variant thereof is intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements not only includes those elements, but also includes other elements not clearly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of more restrictions, the elements limited by the sentence "comprising one..." do not exclude the existence of other identical elements in the process, method, article or equipment including the elements.
[0094] Although the present invention has been disclosed above by the description of the specific embodiments of the present invention, it should be understood that those skilled in the art can design various modifications, improvements or equivalents of the present invention within the spirit and scope of the attached scheme. These modifications, improvements or equivalents should also be considered to be included in the scope of protection claimed by the present invention.
Claims
1. A low silver mixed graphene ink for printed radio frequency identification tags, It is characterized in that The slurry composition is as follows by weight: 2 parts of silver paste and 3-8 parts of pasty graphene ink; wherein, The paste-like graphene ink comprises 6-12 wt % of graphene micro / nano sheets, 0.6-1 wt % of cellulose acetate butyrate, and the remainder is an organic solvent; The silver paste is composed of a silver micro-flake organic carrier and silver micro-flakes in a mass ratio of 1:
3.
2. The low silver mixed graphene ink according to claim 1, It is characterized in that The size of the silver micro-sheet is 0.5-1 μm, and the size of the graphene micro- / nano-sheet is 0.5-1.2 μm.
3. The low silver mixed graphene ink according to claim 1, It is characterized in that In the pasty graphene ink, the organic solvent is selected from at least one of dihydro-levulinic acid ketone, n-methyl pyrrolidone and dimethylformamide.
4. The low silver mixed graphene ink according to any one of claims 1 to 3, It is characterized in that The organic solvent is dihydro-levulinic acid ketone. In the slurry composition, the content of dihydro-levulinic acid ketone ranges from 50 to 72%, the content of the silver microsheets is 15 to 20%, and the content of the graphene micro / nanosheets is 6 to 8%.
5. The low silver mixed graphene ink according to claim 1, It is characterized in that The silver micro-sheet organic carrier is composed of polyurethane resin, diethylene glycol butyl ether, methyl hexachloride curing agent and 3-(trimethoxymethylsilyl) propyl methacrylate in a mass ratio of 1:1:0.5:0.
1.
6. The low silver mixed graphene ink according to any one of claims 1-3 and 5, It is characterized in that The silver paste is further added with the silver micro-sheet organic carrier and the silver micro-sheet mass and 0.8-1.2% of cysteamine.
7. A method for preparing low silver mixed graphene ink, It is characterized in that The steps include: S1, preparation of a paste-like graphene ink: dissolving dried graphene micro / nano sheets in dihydro-L-glucose ketone, adding cellulose acetate butyrate, and stirring to form a paste-like graphene ink; in the paste-like graphene ink, the content of the graphene micro / nano sheets is 6-12wt%, and the content of the cellulose acetate butyrate is 0.6-1wt%; S2, preparation of silver paste: firstly, polyurethane resin, diethylene glycol butyl ether, methyl hexachloride curing agent and 3-(trimethoxymethylsilyl) propyl methacrylate are mixed in a weight ratio of 1:1:0.5:0.1, and stirred to form a silver micro-sheet organic carrier; the silver micro-sheet organic carrier and the silver micro-sheets are mixed and stirred to form a coarse silver paste, wherein the weight ratio of the organic carrier to the silver micro-sheets in the coarse silver paste is 1:3; the coarse silver paste is subjected to roller grinding and filtering to form a silver paste; S3, preparation of low silver mixed graphene ink: mixing the silver paste obtained in step S2 and the paste-like graphene ink obtained in step S1 in a weight ratio of 2:3-8, stirring, and standing in a vacuum oven at room temperature to form the low silver mixed graphene ink.
8. The method for preparing the low silver mixed graphene ink according to claim 7, It is characterized in that Before step S3, a silver paste modification step is also included, in which cysteamine is added to the silver paste obtained in step S2 for modification, and the amount of cysteamine added is 0.8-1.2% of the total mass of the silver microsheet organic carrier and the silver microsheet.
9. The method for preparing the low silver mixed graphene ink according to claim 7 or 8, It is characterized in that In step S1, the method for preparing graphene micro / nano sheets comprises the following steps: S11, placing 75 mesh expandable organic intercalated graphite in a microwave oven at 800W for 30s to achieve graphite expansion; S12, the expanded graphite is dissolved in dihydro-L-glucose ketone at a concentration of 10 mg / ml, and the mixed solution is placed in a 180W, 40kHz ultrasonic pool for 15 hours to perform graphene micro / nanosheet exfoliation. During the exfoliation process, ice cubes are continuously added to the ultrasonic pool to prevent graphite oxidation; S13, the graphene solution after stripping is centrifuged at 300 rpm for 10 minutes, the supernatant is taken, and passed through a 300-mesh steel sieve, and the process is repeated 3 times to remove large particles that have not been stripped, thereby forming a graphene dispersion; S14, the dispersion is centrifuged at 2000 rpm, the graphene sediment is taken out, and dried to obtain the graphene micro / nano sheets.
10. The method for preparing the low silver mixed graphene ink according to claim 7 or 8, It is characterized in that The size of silver microplatelets is 0.5-1 μm, and the size of graphene micro / nanoplatelets is 0.5-1.2 μm.
11. The method for preparing the low silver mixed graphene ink according to claim 7 or 8, It is characterized in that In step S2, stirring at 1000 rpm for 1 hour to form the silver micro-sheet organic carrier; when mixing the silver micro-sheet organic carrier and the silver micro-sheet, the silver micro-sheet is added in batches; the crude silver paste is subjected to a three-roll mill grinding treatment for 3 times, and passed through a 300-mesh filter to form the silver paste; In step S3, the silver paste and the pasty graphene ink are stirred at 500 rpm for 1 hour, and then left to stand at room temperature in a vacuum oven for 3 hours to form the low silver mixed graphene ink.
12. The method for preparing the low silver mixed graphene ink according to claim 11, It is characterized in that In step S2, the batch addition is as follows: first mix the organic carrier and the silver microflakes in a 1:1 weight ratio, stir at 3000 rpm for 30 minutes, add the same amount of silver microflakes, stir for another 30 minutes, add the same amount of silver microflakes again, and continue stirring for 2 hours to form a coarse silver paste, at which time the ratio of silver microflakes to the organic carrier in the coarse silver paste is 75:
25.
13. A printed radio frequency identification tag of low silver mixed graphene, It is characterized in that The low-silver mixed graphene ink is prepared according to any one of claims 1 to 6.
14. A method for preparing a printed radio frequency identification tag of low silver mixed graphene as claimed in claim 13, It is characterized in that include: First, the antenna structure was printed onto the substrate using a 200 mesh screen printer. o C drying for 30 minutes; Secondly, the antenna structure is placed at 165 o C. Metal roller pressing twice under 6MPa; Then, glue is dispensed using a glue dispenser, and the chip is welded in the center of the antenna using a packaging machine. o C. After 15 seconds of hot pressing, the RFID tag is formed; The substrate is selected from any one of TPU, coated paper, non-woven fabric, glass, and PET.
Citation Information
Patent Citations
Method for preparing water-soluble precious metal nano particles
CN103962563A
Conductive silver paste and preparation method thereof
CN106297950A
Cladding material for improving surface electric conductivity of industrial graphene nanoplatelets and preparation method of cladding material
CN107159884A
Graphene-silver composite RFID tag and preparation method and application thereof
CN114639504A
Conductive silver paste and preparation method thereof
CN117809883A
Cited By
Printed radio frequency identification tag and preparation method thereof
CN119623503A
Radio frequency identification tag and manufacturing method thereof
CN119990173A