Tb-Al-MOG coated PU fluorescent material and preparation method thereof
Through the preparation method of Tb-Al-MOG@PU material, the problems of instability and insufficient molding capacity of MOFs materials in water bodies are solved, and high stability and efficient fluorescence detection performance are achieved, which is suitable for a variety of solution environments.
Patent Information
- Application Number
- CN202411202954.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-29
AI Technical Summary
Traditional MOFs materials are unstable in water bodies, easily settle, and have low molding capacity and recycling rate, which affect detection accuracy and repeatability.
Using the preparation method of Tb-Al-MOG@PU fluorescent material, Tb(NO3)3·6H2O, Al(NO3)3·9H2O and 1,3,5-phenyltriacetic acid in N,N-dimethyl Dissolve in formamide, add polyurethane to form a viscous solution, condense and reflux, and cure in the mold to obtain a Tb-Al-MOG@PU block-like porous solid material, enhancing its molding ability and water stability.
Improve the stability and molding capacity of MOGs materials in water bodies, achieve low detection limit (0.03μM) and high repeat detection accuracy, high fluorescence responsiveness and reusability, suitable for a variety of salts and organic contaminations in solution.
Smart Images

Figure CN119039967A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional material composites, and in particular relates to a Tb-Al-MOG@PU fluorescent material and a preparation method thereof. Background Art
[0002] Fluorescence sensors have attracted much attention due to their high sensitivity, intuitive detection reaction phenomena and easy operation. Designing and synthesizing corresponding fluorescence sensors will become an indispensable technology in future development.
[0003] The detection of water pollutants is a very important part of environmental protection. Fluorescent sensing materials that meet the requirements of fluorescent detection of water pollutants need to have excellent water stability and recyclability. Rare earth metal organic frameworks (RE-MOFs) have excellent fluorescence detection performance. However, most MOFs materials synthesized by traditional hydrothermal methods are powder particles. During the detection process, the MOF powder needs to be evenly dispersed in the water environment to be tested under ultrasonic conditions, and then an appropriate amount of water to be tested is placed in the optical path to measure the luminescence behavior of the fluorescent MOF. Therefore, the uniform and stable dispersion of fluorescent MOF in water is an important guarantee for obtaining accurate detection results. However, due to the effect of gravity, nano-MOFs powder will gradually settle at the bottom of the detection system during the detection process, resulting in a reduction in the effective fluorescent MOF powder in the optical path and test errors. In addition, the recycling rate of MOF powder is low. The dispersion and recovery of MOF are two contradictory processes. The better the dispersion, the more difficult the recovery. It is usually necessary to collect MOF again with the help of centrifugation and poor solvent exchange, but its recovery rate is still not high. In summary, MOF powder is not conducive to practical application environment.
[0004] Even if MOF is made into a gel block MOG with the help of Al-MOG gel, its molding ability still depends on the stability of Al-MOG and the interfacial bonding strength between Al-MOG and MOF. In essence, Al-MOG is still a metal-organic hybrid material. Although its molding ability is much better than that of MOF powder, it still has a big gap compared with organic polymers. Therefore, how to prepare MOG materials with efficient luminescent centers, excellent molding ability and stability is an urgent problem to be solved. Summary of the invention
[0005] The purpose of the present invention is to provide a Tb-Al-MOG@PU fluorescent material and a preparation method to solve the problems of stability and molding ability of existing MOGs materials in water.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for preparing a Tb-Al-MOG@PU fluorescent material, comprising:
[0008] S1: Dissolve Tb(NO3)3·6H2O, Al(NO3)3·9H2O and 1,3,5-tricresyl acid in N,N-dimethylformamide and stir until clear, which is referred to as solution A;
[0009] S2: dissolving polyurethane in N,N-dimethylformamide and stirring until clear, which is referred to as solution B;
[0010] S3: Heat solution A with stirring. When heated to 120°C, add solution B into solution A, continue heating and stirring, condense and reflux, and form a viscous solution C;
[0011] S4: pouring the viscous solution C into a mold to cool and solidify, thereby obtaining a Tb-Al-MOG@PU block-shaped porous solid fluorescent material;
[0012] S5: washing the Tb-Al-MOG@PU block porous solid fluorescent material and drying it to obtain the Tb-Al-MOG@PU fluorescent material.
[0013] Preferably, the amounts of Tb(NO3)3·6H2O, Al(NO3)3·9H2O, 1,3,5-tricresyl acid and N,N-dimethylformamide in S1 are 3-5 mmol, 3-5 mmol, 5-7 mmol and 30-40 mL respectively.
[0014] Preferably, in S2, 0.1-1 wt% of polyurethane by mass fraction of the total mass is dissolved in 5-15 mL of N,N-dimethylformamide.
[0015] Preferably, in S3, solution A is transferred into a round-bottom flask, heated in an oil bath, and stirred.
[0016] Preferably, in S3, after adding solution B and heating, condensation and reflux are performed for 4 to 6 hours to form a viscous solution C.
[0017] Preferably, in S4, the curing is a two-step curing: first, drying and molding in an oven at 50°C; then secondary curing at 120°C, to finally obtain the Tb-Al-MOG@PU block-shaped porous solid fluorescent material.
[0018] Preferably, the molding is first dried in an oven at 50° C. for 24 to 36 hours; and then secondary curing is performed at 120° C. for 4 hours.
[0019] Preferably, in S5, the obtained Tb-Al-MOG@PU block porous solid fluorescent material is soaked in distilled water, vacuum dried at 105°C to remove the solvent in the gel pores, and then dried in an oven at 50°C to obtain the Tb-Al-MOG@PU fluorescent material.
[0020] Preferably, in S5, the mixture is immersed in distilled water for 1 hour, vacuum dried for 30 minutes, and dried in an oven at 50° C. for 2 days.
[0021] A Tb-Al-MOG@PU fluorescent material is prepared by the preparation method according to any one of claims 1 to 9.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The preparation method of the present invention introduces polyurethane PU. In the sol-gel process, the mutual cross-linking of the PU long molecular chains is also more conducive to the formation of gel, which increases the resistance of the MOF coordination effect. At the same time, the hydrogen bonds inside the PU soft segment are dissociated, and instead generate stronger hydrogen bonds with the gel system, which further inhibits the growth rate of MOFs crystals, is more conducive to the formation of gel structure, enhances the gel network strength, and ultimately enhances the molding ability and water stability of Tb-Al-MOG@PU.
[0024] The Tb-Al-MOG@PU block porous solid material prepared by the present invention has significant recognition and detection performance of chlortetracycline in water, with a detection limit (LOD) as low as 0.03 μM, and an error of only 2.6% after 30 repeated tests. It shows high fluorescence responsiveness, high stability, and reusability, and can stably exist in a variety of salt solutions and organic pollution solutions. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0026] Figure 1 This is the XRD pattern of Tb-Al-MOG@PU synthesized in the present invention;
[0027] Figure 2 This is a SEM image of Tb-Al-MOG@PU synthesized in the present invention;
[0028] Figure 3These are pictures of Tb-Al-MOG@PU synthesized in the present invention, (a) optical picture under natural light; (b) luminescent picture under 365nm wavelength; (c) luminescent picture under 280nm wavelength. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.
[0030] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.
[0032] In the description of the embodiments of the present invention, it should be noted that if the terms "upper", "lower", "horizontal", "inner", etc. indicate an orientation or positional relationship based on the orientation or positional relationship shown in the drawings, or the orientation or positional relationship in which the product of the invention is usually placed when in use, it is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, the terms "first", "second", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.
[0033] In addition, if the term "horizontal" appears, it does not mean that the component is required to be absolutely horizontal, but can be slightly tilted. For example, "horizontal" only means that its direction is more horizontal than "vertical", which does not mean that the structure must be completely horizontal, but can be slightly tilted.
[0034] In the description of the embodiments of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal connection of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0035] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0036] The present application discloses a method for preparing a Tb-Al-MOG@PU fluorescent material, comprising:
[0037] S1: Dissolve Tb(NO3)3·6H2O, Al(NO3)3·9H2O and 1,3,5-tricresyl acid in N,N-dimethylformamide and stir until clear, which is referred to as solution A;
[0038] S2: dissolving polyurethane in N,N-dimethylformamide and stirring until clear, which is referred to as solution B;
[0039] S3: Heat solution A with stirring. When heated to 120°C, add solution B into solution A, continue heating and stirring, condense and reflux, and form a viscous solution C;
[0040] S4: pouring the viscous solution C into a mold to cool and solidify, thereby obtaining a Tb-Al-MOG@PU block-shaped porous solid fluorescent material;
[0041] S5: washing the Tb-Al-MOG@PU block porous solid fluorescent material and drying it to obtain the Tb-Al-MOG@PU fluorescent material.
[0042] Not all MOFs and MOGs can be tightly combined together, so the introduction of long-chain polymers (such as polyurethane PU, polystyrene PS, etc.) can enhance the hydrogen bonding of the system during the sol-gel process, inhibit the growth rate of MOFs crystals, and be more conducive to the formation of gel structure and enhance the strength of the gel network, thereby improving the stability and molding ability of MOGs materials in water. This is of great significance for the synthesis of large-size MOGs functional materials and high-performance MOGs fluorescent sensing materials.
[0043] In some embodiments, a method for preparing a Tb-Al-MOG@PU fluorescent material comprises the following steps:
[0044] Step 1: Weigh 3-5 mmol Tb(NO3)3·6H2O, 3-5 mmol Al(NO3)3·9H2O and 5-7 mmol 1,3,5-tricarboxylic acid (H3BTC), dissolve in 30-40 mL N,N-dimethylformamide, and stir until clear. This is referred to as solution A.
[0045] Step 2: Weigh 0.1-1 wt% polyurethane (PU) with a mass fraction of the total mass, dissolve it in 5-15 mL N,N-dimethylformamide, and stir until clear, which is recorded as solution B.
[0046] Step 3: Transfer solution A into a round-bottom flask and heat with stirring. When the oil bath is heated to 120°C, add solution B into the round-bottom flask and continue heating with stirring. Condensation and reflux are performed for 4 to 6 hours to form a viscous solution C.
[0047] Step 4: Pour the viscous solution C into a 3 cm × 3 cm silicone mold with a thickness of 1 cm, quickly cool it to room temperature, and then perform two-step curing: first dry it in a 50 ° C oven for 24 to 36 hours; then perform secondary curing at 120 ° C for 4 hours to finally obtain the Tb-Al-MOG@PU block porous solid fluorescent material.
[0048] Step 5: Soak the obtained Tb-Al-MOG@PU block porous solid fluorescent material in distilled water for 1 hour, vacuum dry it at 105°C for 30 minutes to remove the solvent in the gel pores, and then dry it in an oven at 50°C for about 2 days to obtain the Tb-Al-MOG@PU fluorescent material.
[0049] Embodiment 1:
[0050] Step 1: Weigh 3 mmol Tb(NO3)3·6H2O, 3 mmol Al(NO3)3·9H2O and 6 mmol 1,3,5-tricarboxylic acid (H3BTC), dissolve in 30 mL N,N-dimethylformamide, and stir until clear. This is referred to as solution A.
[0051] Step 2: Weigh 0.1 wt% polyurethane (PU) with a mass fraction of the total mass, dissolve it in 5 mL N,N-dimethylformamide, and stir until clear, which is recorded as solution B.
[0052] Step 3: Transfer solution A into a round-bottom flask and heat with stirring. When the oil bath is heated to 120°C, add solution B into the round-bottom flask and continue heating with stirring. Condensation and reflux for 4 hours to form a viscous solution C.
[0053] Step 4: Pour the viscous solution C into a 3 cm × 3 cm silicone mold with a thickness of 1 cm, quickly cool it to room temperature, and then perform two-step curing: first dry it in a 50 ° C oven for 24 hours; then perform secondary curing at 120 ° C for 4 hours to finally obtain the Tb-Al-MOG@PU block porous solid fluorescent material.
[0054] Step 5: Soak the obtained Tb-Al-MOG@PU block porous solid fluorescent material in distilled water for 1 hour, vacuum dry it at 105°C for 30 minutes to remove the solvent in the gel pores, and then dry it in an oven at 50°C for about 2 days to obtain the Tb-Al-MOG@PU fluorescent material.
[0055] Embodiment 2:
[0056] Step 1: Weigh 4.5 mmol Tb(NO3)3·6H2O, 4.5 mmol Al(NO3)3·9H2O and 6 mmol 1,3,5-tricarboxylic acid (H3BTC), dissolve in 35 mL N,N-dimethylformamide, and stir until clear. This is referred to as solution A.
[0057] Step 2: Weigh 0.5 wt% polyurethane (PU) with a mass fraction of the total mass, dissolve it in 10 mL N,N-dimethylformamide, and stir until clear, which is recorded as solution B.
[0058] Step 3: Transfer solution A into a round-bottom flask and heat with stirring. When the oil bath is heated to 120°C, add solution B into the round-bottom flask and continue heating with stirring. Condensation and reflux for 4 hours to form a viscous solution C.
[0059] Step 4: Pour the viscous solution C into a 3 cm × 3 cm silicone mold with a thickness of 1 cm, quickly cool it to room temperature, and then perform two-step curing: first, dry it in a 50 ° C oven for 36 hours; then perform secondary curing at 120 ° C for 4 hours to finally obtain the Tb-Al-MOG@PU block porous solid fluorescent material.
[0060] Step 5: Soak the obtained Tb-Al-MOG@PU block porous solid fluorescent material in distilled water for 1 hour, vacuum dry it at 105°C for 30 minutes to remove the solvent in the gel pores, and then dry it in an oven at 50°C for about 2 days to obtain the Tb-Al-MOG@PU fluorescent material.
[0061] Embodiment 3:
[0062] Step 1: Weigh 3 mmol Tb(NO3)3·6H2O, 3 mmol Al(NO3)3·9H2O and 6 mmol 1,3,5-tricarboxylic acid (H3BTC), dissolve in 40 mL N,N-dimethylformamide, and stir until clear. This is referred to as solution A.
[0063] Step 2: Weigh 1 wt% of polyurethane (PU) with a mass fraction of the total mass, dissolve it in 10 mL of N,N-dimethylformamide, and stir until clear, which is recorded as solution B.
[0064] Step 3: Transfer solution A into a round-bottom flask and heat with stirring. When the oil bath is heated to 120°C, add solution B into the round-bottom flask and continue heating with stirring. Condensation and reflux are performed for 5 hours to form a viscous solution C.
[0065] Step 4: Pour the viscous solution C into a 3 cm × 3 cm silicone mold with a thickness of 1 cm, quickly cool it to room temperature, and then perform two-step curing: first, dry it in a 50 ° C oven for 36 hours; then perform secondary curing at 120 ° C for 4 hours to finally obtain the Tb-Al-MOG@PU block porous solid fluorescent material.
[0066] Step 5: Soak the obtained Tb-Al-MOG@PU block porous solid fluorescent material in distilled water for 1 hour, vacuum dry it at 105°C for 30 minutes to remove the solvent in the gel pores, and then dry it in an oven at 50°C for about 2 days to obtain the Tb-Al-MOG@PU fluorescent material.
[0067] See also Figure 1 ,The X-ray powder diffraction pattern of Tb-Al-MOG@PU shows that Tb-Al-MOG@PU has good crystallinity, which can ensure the luminescence performance of the central Tb.
[0068] See also Figure 2 ,Scanning electron microscope photo of Tb-Al-MOG@PU, it can be seen that Tb-MOF is tightly wrapped by the matrix of Al-MOG and PU to form a dense structure, providing better structural stability.
[0069] See also Figure 3 (a) Optical image of Tb-Al-MOG@PU under natural light; indicating that Tb-Al-MOG@PU has good molding ability; (b) is the luminescence image under 365nm wavelength; (c) is the luminescence image under 280nm wavelength. It can emit green fluorescence under 365nm and 280nm wavelength ultraviolet light, and has good fluorescence luminescence performance.
[0070] In summary, the present invention discloses a Tb-Al-MOG@PU fluorescent material and a preparation method. By introducing polyurethane PU, in the sol-gel process, the mutual cross-linking of the PU long molecular chains is conducive to the formation of gel, the hydrogen bonds inside the PU soft segment are dissociated, and a strong hydrogen bond effect is generated with the gel system, which further inhibits the MOFs crystal growth rate, is more conducive to the gel network strength, and finally enhances the molding ability and water stability of Tb-Al-MOG@PU. The Tb-Al-MOG@PU block porous solid material prepared by the present invention has significant recognition and detection performance of chlortetracycline in water, with a detection limit (LOD) as low as 0.03μM, and an error of only 2.6% after repeated detection for 30 times, showing high fluorescence responsiveness, high stability, and reusability, and can stably exist in a variety of salt solutions and organic pollution solutions.
[0071] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a Tb-Al-MOG@PU fluorescent material, characterized in that: include: S1: Dissolve Tb(NO3)3·6H2O, Al(NO3)3·9H2O and 1,3,5-tricresyl acid in N,N-dimethylformamide and stir until clear, which is referred to as solution A; S2: dissolving polyurethane in N,N-dimethylformamide and stirring until clear, which is referred to as solution B; S3: Heat solution A with stirring. When heated to 120°C, add solution B into solution A, continue heating and stirring, condense and reflux, and form a viscous solution C; S4: pouring the viscous solution C into a mold to cool and solidify, thereby obtaining a Tb-Al-MOG@PU block-shaped porous solid fluorescent material; S5: washing the Tb-Al-MOG@PU block porous solid fluorescent material and drying it to obtain the Tb-Al-MOG@PU fluorescent material.
2. The method for preparing a Tb-Al-MOG@PU fluorescent material according to claim 1, characterized in that: The amounts of Tb(NO3)3·6H2O, Al(NO3)3·9H2O, 1,3,5-tricresyl acid and N,N-dimethylformamide in S1 are 3-5 mmol, 3-5 mmol, 5-7 mmol and 30-40 mL respectively.
3. The method for preparing a Tb-Al-MOG@PU fluorescent material according to claim 1, characterized in that: In the S2, 0.1-1 wt% of polyurethane with a mass fraction of the total mass is dissolved in 5-15 mL of N,N-dimethylformamide.
4. The method for preparing a Tb-Al-MOG@PU fluorescent material according to claim 1, characterized in that: In S3, solution A is transferred into a round-bottom flask, heated in an oil bath, and stirred.
5. The method for preparing a Tb-Al-MOG@PU fluorescent material according to claim 1, characterized in that: In the S3, solution B is added, heated, and then condensed and refluxed for 4 to 6 hours to form a viscous solution C.
6. The method for preparing a Tb-Al-MOG@PU fluorescent material according to claim 1, characterized in that: In S4, the curing is a two-step curing: first, drying and forming in an oven at 50° C.; then secondary curing at 120° C., and finally obtaining a Tb-Al-MOG@PU block-shaped porous solid fluorescent material.
7. The method for preparing a Tb-Al-MOG@PU fluorescent material according to claim 6, characterized in that: First, the mold is dried in an oven at 50°C for 24 to 36 hours; then, a secondary curing is performed at 120°C for 4 hours.
8. The method for preparing a Tb-Al-MOG@PU fluorescent material according to claim 1, characterized in that: In S5, the obtained Tb-Al-MOG@PU block porous solid fluorescent material is soaked in distilled water, vacuum dried at 105° C. to remove the solvent in the gel pores, and then dried in an oven at 50° C. to obtain the Tb-Al-MOG@PU fluorescent material.
9. The method for preparing a Tb-Al-MOG@PU fluorescent material according to claim 1, characterized in that: In the S5, the sample was immersed in distilled water for 1 hour, vacuum dried for 30 minutes, and dried in an oven at 50° C. for 2 days.
10. A Tb-Al-MOG@PU fluorescent material, characterized in that: The method is prepared by any one of claims 1 to 9.
Citation Information
Cited By
Preparation method of polyurethane sponge supported MOG material
CN119192669A