Efficient green gold leaching agent and application method thereof

Through the high-efficiency green gold-leaching agent composed of thiobenzenesulfonate, aid infusion agent and mild oxidizing agent, the problems of environmental pollution and high reagent consumption in the existing gold extraction technology are solved, and the rapid and low-cost gold extraction effect is achieved. Suitable for a variety of gold ores.

CN119040628APending Publication Date: 2024-11-29CENT SOUTH UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411188380.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing cyanation method and non-cyanolytic gold-leaching agents have problems such as environmental pollution, high reagent consumption, long leaching cycle, high cost and poor ore adaptability during the gold extraction process, which limits their industrial application.

Method used

Use high-efficiency green gold-implanted agent composed of thiobenzenesulfonate, aid infusion agent and gentle oxidizing agent, and prepares it through mixing and compounding. It is suitable for a wide pH range, and combines metal salts and complexing agents to promote oxidative dissolution of gold. It is suitable for Different types of gold ore.

Benefits of technology

It achieves non-toxic, low energy consumption, high rapid gold impregnation efficiency, low reagent consumption, environmentally friendly gold extraction effect, strong applicability, and supports the recycling of leaching liquid.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an efficient green gold leaching agent and an application method thereof. The efficient green gold leaching agent is prepared by uniformly mixing and compounding a proper amount of thiobenzene sulfonate, a leaching aid and a mild oxidizing agent. The application method of the efficient green gold leaching agent comprises the following steps that a gold ore raw material is ground, and the part with the particle size smaller than 74 microns in the gold ore raw material accounts for 90 wt% or above; the concentration of the gold ore pulp is adjusted to be 30%-50%, then a proper amount of the efficient green gold leaching agent is added, then the pH value of the gold ore pulp is adjusted to be 5-11, and finally stirring leaching is conducted for 3-24 hours at the normal temperature and the normal pressure. According to the efficient green gold leaching agent and the application method thereof, the efficient green gold leaching agent is formed by directly and evenly mixing and compounding common non-toxic environment-friendly chemical reagents, the preparation method is simple, the adaptability to different types of ores is high, and efficient gold leaching can be achieved within the wide pH range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hydrometallurgy, and in particular to a high-efficiency green gold leaching agent and an application method thereof. Background Art

[0002] Since the 19th century, cyanide has become the main process for gold extraction due to its mature technology and simple process. However, it has the following major defects: (1) Cyanide is highly toxic and harmful to the environment; (2) The leaching rate is slow, and the leaching cycle is usually as long as 36-48 hours; (3) The treatment of cyanide tailings is also a major problem. At present, it is mainly piled in tailings dams. This will not only release harmful substances in the tailings into the surrounding soil and water resources, but also consume a lot of space to build tailings dams. Therefore, the development of non-cyanide gold leaching agents is imminent. The non-cyanide gold leaching agents that have been studied more include thiosulfate, thiourea, thiocyanate, halogen, etc. The leaching process of thiosulfate, thiourea and thiocyanate all has the problem of high reagent consumption. The halogen method mainly includes chlorination, bromination and iodination. Chlorination causes serious corrosion to the equipment under acidic conditions, and the chlorine gas generated during the leaching process is harmful to the environment; compared with chlorination, bromination and iodination have better gold leaching effects, but their costs are relatively high. The above problems seriously limit the industrial application of these non-cyanide gold leaching agents.

[0003] In recent years, some new synthetic gold leaching agents such as "Golden Cicada" have appeared on the market, which have initially demonstrated the advantages of non-toxic / low-toxic environmental protection, fast gold leaching rate, and high gold recovery rate, and have attracted the attention of more and more researchers and technical personnel of gold companies. However, the synthesis of existing new synthetic gold leaching agents requires a pyro-roasting process, which requires a large amount of fuel and energy, and easily leads to environmental pollution. In addition, there is a common problem of high energy consumption in the pyro-roasting process, which makes the synthesis cost of the gold leaching agent high and the process complicated. Cyanide can still be detected in some synthetic gold leaching agents currently on the market, and their ore adaptability is poor, and large-scale industrial application has not yet been achieved. Therefore, the research and development of green and efficient non-cyanide gold leaching agents is still an urgent problem for gold companies. Summary of the invention

[0004] In order to solve the technical problems in the above-mentioned background technology, the present invention provides a high-efficiency green gold leaching agent and an application method thereof. The method has high gold leaching efficiency, a wide applicable pH range, and strong ore adaptability.

[0005] The invention provides a high-efficiency green gold leaching agent, which is prepared by mixing and compounding appropriate amounts of thiobenzenesulfonate, a leaching aid and a mild oxidant.

[0006] In a preferred embodiment of the high-efficiency green gold leaching agent provided by the present invention, the mass ratio of the thiobenzenesulfonate, the leaching aid and the mild oxidant is 100:(0.05-0.5):(10-20).

[0007] In a preferred embodiment of the high-efficiency green gold leaching agent provided by the present invention, the thiobenzenesulfonate is sodium thiobenzenesulfonate or potassium thiobenzenesulfonate.

[0008] In a preferred embodiment of the high-efficiency green gold leaching agent provided by the present invention, the leaching aid is at least one of thiocyanate, thiourea and glycine.

[0009] In a preferred embodiment of the high-efficiency green gold leaching agent provided by the present invention, the thiocyanate is sodium thiocyanate or potassium thiocyanate, and the glycine is sodium glycine or potassium glycine.

[0010] In a preferred embodiment of the high-efficiency green gold leaching agent provided by the present invention, the mild oxidant includes a metal salt and a complexing agent.

[0011] In a preferred embodiment of the high-efficiency green gold leaching agent provided by the present invention, the metal salt includes one of an iron salt, a copper salt, a nickel salt, and a cobalt salt.

[0012] In a preferred embodiment of the high-efficiency green gold leaching agent provided by the present invention, the complexing agent includes one or more of a citrate-containing compound, a salicylate-containing compound, a sulfosalicylate-containing compound, a cyclohexanediaminetetraacetate-containing compound, and a hydroxyethylethylenediaminetriacetate-containing compound; preferably, the citrate-containing compound is sodium citrate or potassium citrate, the salicylate-containing compound is sodium salicylate or potassium salicylate, the sulfosalicylate-containing compound is sodium sulfosalicylate or potassium sulfosalicylate, the cyclohexanediaminetetraacetate-containing compound is sodium cyclohexanediaminetetraacetate or potassium cyclohexanediaminetetraacetate, and the hydroxyethylethylenediaminetriacetate-containing compound is sodium hydroxyethylethylenediaminetriacetate or potassium hydroxyethylethylenediaminetriacetate.

[0013] In a preferred embodiment of the high-efficiency green gold leaching agent provided by the present invention, the molar ratio of the metal ions in the metal salt to the complexing agent is 1:(1.2-7).

[0014] The present invention also provides an application method of a high-efficiency green gold leaching agent, comprising the following steps: grinding a gold ore raw material so that the portion of the gold ore raw material with a particle size less than 74 μm accounts for more than 90 wt %; adjusting the gold ore slurry concentration to 30%-50%, then adding an appropriate amount of the high-efficiency green gold leaching agent, and then adjusting the pH value of the gold ore slurry to 5-11, and finally stirring and leaching for 3-24 hours at normal temperature and pressure.

[0015] In a preferred embodiment of the application method of the high-efficiency green gold leaching agent provided by the present invention, the addition amount of the high-efficiency green gold leaching agent is 0.2wt%-5wt% of the weight of the gold ore slurry.

[0016] The high-efficiency green gold leaching agent prepared by the present invention has a synergistic gold leaching effect of thiobenzenesulfonate and a leaching aid, forms a stable mixed ligand complex with gold, and the metal complex ions formed by the metal salt and the complexing agent continuously promote the oxidation and dissolution of gold as an oxidant. The gold leaching agent prepared by the present invention can be used in a wide pH range (5-11), which makes the gold leaching agent prepared by the present invention highly applicable. From the spatial structure of the metal complex ion, it can be seen that the central metal atom is tightly bound by the complexing agent, which can significantly reduce the oxidation of the metal ions to the thiobenzenesulfonate and the leaching aid, thereby improving the stability of the leaching agent. In addition, the thiobenzenesulfonate has high stability and low reagent consumption, and the recycling of the leaching solution can be realized.

[0017] Compared with the prior art, the efficient green gold leaching agent and its application method provided by the present invention have the following beneficial effects:

[0018] 1. The high-efficiency green gold leaching agent provided by the present invention is non-toxic, environmentally friendly, and has a simple preparation process. It only requires directly mixing and compounding several existing thiobenzenesulfonates, leaching aids and mild oxidants. It has low requirements on preparation equipment and is suitable for large-scale promotion and application.

[0019] 2. The leaching pH range of the high-efficiency green gold leaching agent prepared by the present invention is 5-11, and the leaching pH range is wide.

[0020] 3. The high-efficiency green gold leaching agent prepared by the present invention has a fast gold leaching rate, high efficiency, strong adaptability to different types of ores, and low reagent consumption, which is conducive to the recycling of the leaching solution. DETAILED DESCRIPTION

[0021] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] Gold mine raw material 1: This gold mine is a typical quartz-type gold mine with a gold grade of 4.49 g / t. The main gangue component is SiO2, accounting for 74.6% of the gold mine composition, and Al2O3 accounts for 6.32%.

[0023] Embodiment 1:

[0024] Preparation of an efficient green gold leaching agent: Sodium thiobenzenesulfonate, potassium thiocyanate and a mild oxidant are mixed at a mass ratio of 100:0.05:10 to prepare the efficient green gold leaching agent; wherein the mild oxidant is ferric sulfate and sodium salicylate, and the molar ratio thereof is 1:1.2.

[0025] The gold ore raw material 1 is finely ground until the portion of the gold ore raw material 1 with a particle size less than 74 μm accounts for more than 90 wt %, the gold ore slurry concentration is adjusted to 30%, and then 0.2 wt % of the high-efficiency green gold leaching agent is added, the pH of the gold ore slurry is adjusted to 10, and leaching is carried out under stirring at room temperature and pressure, the stirring speed is 300 r / min, the leaching time is 8 hours, and the leaching results are: the gold leaching rate is 90.7%, and the leaching agent consumption is 5.46 kg / t-ore.

[0026] Embodiment 2:

[0027] Preparation of an efficient green gold leaching agent: First, sodium thiobenzenesulfonate, thiourea and a mild oxidant are mixed at a mass ratio of 100:0.2:15 to prepare the efficient green gold leaching agent; wherein the mild oxidant is nickel sulfate and sodium citrate, and the molar ratio thereof is 1:1.2.

[0028] The gold ore raw material 1 is finely ground until the portion of the gold ore raw material 1 with a particle size less than 74 μm accounts for more than 90 wt %, the gold ore slurry concentration is adjusted to 30%, and then 0.3 wt % of the high-efficiency green gold leaching agent is added, the pH of the gold ore slurry is adjusted to 8, and leaching is carried out under stirring at room temperature and pressure, the stirring speed is 300 r / min, the leaching time is 8 hours, and the leaching results are: the gold leaching rate is 91.6%, and the leaching agent consumption is 5.75 kg / t-ore.

[0029] Embodiment 3:

[0030] Preparation of an efficient green gold leaching agent: First, sodium thiobenzenesulfonate, thiourea and a mild oxidant are mixed at a mass ratio of 100:0.5:20 to prepare the efficient green gold leaching agent; wherein the mild oxidant is cobalt sulfate and glycine, and the molar ratio thereof is 1:3.2.

[0031] The gold ore raw material 1 is finely ground until the portion of the gold ore raw material 1 with a particle size less than 74 μm accounts for more than 90 wt %, the gold ore slurry concentration is adjusted to 30%, and then 0.3 wt % of the high-efficiency green gold leaching agent is added, the pH of the gold ore slurry is adjusted to 9, and leaching is carried out under stirring at room temperature and pressure, the stirring speed is 300 r / min, the leaching time is 8 hours, and the leaching results are: the gold leaching rate is 91.3%, and the leaching agent consumption is 5.94 kg / t-ore.

[0032] Gold ore raw material 2: The gold ore is gold concentrate roasted sand with a gold grade of 34.26g / t. The main components are magnetite and hematite, which account for 28.4% and 37.3% of the gold ore composition respectively.

[0033] Embodiment 4:

[0034] Preparation of an efficient green gold leaching agent: Sodium thiobenzenesulfonate, potassium thiocyanate and a mild oxidant are mixed at a mass ratio of 100:0.05:10 to prepare the efficient green gold leaching agent; wherein the mild oxidant is ferric sulfate and sodium salicylate, and the molar ratio thereof is 1:1.2.

[0035] The gold ore raw material 2 is finely ground until the portion of the gold ore raw material 2 with a particle size of less than 74 μm accounts for more than 90 wt %, the gold ore slurry concentration is adjusted to 30%, and then 0.2 wt % of the high-efficiency green gold leaching agent is added, the pH of the gold ore slurry is adjusted to 10, and leaching is carried out under stirring at room temperature and pressure, the stirring speed is 300 r / min, the leaching time is 8 hours, and the leaching results are: the gold leaching rate is 89.4%, and the leaching agent consumption is 7.43 kg / t-ore.

[0036] Embodiment 5:

[0037] Preparation of an efficient green gold leaching agent: First, sodium thiobenzenesulfonate, thiourea and a mild oxidant are mixed at a mass ratio of 100:0.2:15 to prepare the efficient green gold leaching agent; wherein the mild oxidant is nickel sulfate and sodium citrate, and the molar ratio thereof is 1:1.2.

[0038] The gold ore raw material 2 is finely ground until the portion of the gold ore raw material 2 with a particle size less than 74 μm accounts for more than 90 wt %, the gold ore slurry concentration is adjusted to 30%, and then 0.3 wt % of the high-efficiency green gold leaching agent is added, the pH of the gold ore slurry is adjusted to 8, and leaching is carried out under stirring at room temperature and pressure, the stirring speed is 300 r / min, the leaching time is 8 hours, and the leaching results are: the gold leaching rate is 90.3%, and the leaching agent consumption is 7.86 kg / t-ore.

[0039] Embodiment 6:

[0040] Preparation of an efficient green gold leaching agent: First, sodium thiobenzenesulfonate, thiourea and a mild oxidant are mixed at a mass ratio of 100:0.5:20 to prepare the efficient green gold leaching agent; wherein the mild oxidant is cobalt sulfate and glycine, and the molar ratio thereof is 1:3.2.

[0041] The gold ore raw material 2 is finely ground until the portion of the gold ore raw material 2 with a particle size less than 74 μm accounts for more than 90 wt %, the gold ore slurry concentration is adjusted to 30%, and then 0.3 wt % of the high-efficiency green gold leaching agent is added, the pH of the gold ore slurry is adjusted to 9, and leaching is carried out under stirring at room temperature and pressure, the stirring speed is 300 r / min, the leaching time is 8 hours, and the leaching results are: the gold leaching rate is 90.6%, and the leaching agent consumption is 8.16 kg / t-ore.

[0042] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A highly efficient green gold leaching agent, characterized in that: The high-efficiency green gold leaching agent is prepared by mixing and compounding appropriate amounts of thiobenzenesulfonate, a leaching aid and a mild oxidant.

2. The high-efficiency green gold leaching agent according to claim 1, characterized in that: The mass ratio of the thiobenzenesulfonate, the soaking aid and the mild oxidant is 100:(0.05-0.5):(10-20).

3. The high-efficiency green gold leaching agent according to claim 1 or 2, characterized in that: The thiobenzenesulfonate is sodium thiobenzenesulfonate or potassium thiobenzenesulfonate, and the leaching aid is at least one of thiocyanate, thiourea and glycine.

4. The high-efficiency green gold leaching agent according to claim 3, characterized in that: The thiocyanate is sodium thiocyanate or potassium thiocyanate, and the glycine is sodium glycine or potassium glycine.

5. The high-efficiency green gold leaching agent according to claim 1 or 2, characterized in that: The mild oxidants include metal salts and complexing agents.

6. The high-efficiency green gold leaching agent according to claim 5, characterized in that: The metal salt includes one of an iron salt, a copper salt, a nickel salt and a cobalt salt.

7. The high-efficiency green gold leaching agent according to claim 5, characterized in that: The complexing agent includes one or more of a compound containing citrate, a compound containing salicylate, a compound containing sulfosalicylate, a compound containing cyclohexanediaminetetraacetate, and a compound containing hydroxyethylethylenediaminetriacetate.

8. The high-efficiency green gold leaching agent according to claim 5, characterized in that: The molar ratio of the metal ion in the metal salt to the complexing agent is 1:(1.2-7).

9. An application method of the high-efficiency green gold leaching agent according to claim 1, characterized in that: The following steps are involved: The gold ore raw material is ground so that the portion of the gold ore raw material with a particle size of less than 74 μm accounts for more than 90 wt %; the gold ore slurry concentration is adjusted to 30%-50%, and then a proper amount of the high-efficiency green gold leaching agent is added, and then the pH value of the gold ore slurry is adjusted to 5-11, and finally stirred and leached at normal temperature and pressure for 3-24 hours.

10. The high-efficiency green gold leaching agent according to claim 9, characterized in that: The addition amount of the high-efficiency green gold leaching agent is 0.2wt%-5wt% of the weight of the gold ore slurry.

Citation Information

Cited By

  • Process for separating precious metal from copper-nickel smelting waste

    CN121250126A