Electrolyzed water catalyst with photothermal conversion performance as well as preparation method and application
By using biomass waste to prepare porous carbon-supported non-precious metal catalysts, combined with the photothermal conversion performance, the problems of high cost and insufficient energy conversion efficiency of traditional electrolytic catalysts are solved, and efficient electrolytic catalysts are achieved and low-cost solar energy utilization is achieved. , and has the advantages of 'zero carbon' emissions.
Patent Information
- Application Number
- CN202411153110.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
AI Technical Summary
Traditional electrolytic water catalysts have high cost and insufficient overall energy conversion efficiency of non-precious metal catalysts, which hinders the widespread application of electrolytic water hydrogen production, and the environmental pollution in the preparation process of carbon materials is high.
Biomass waste is used to prepare porous carbon-supported non-precious metal electrolytic catalysts, improve the electrolytic catalytic performance through photothermal conversion performance, and prepare lignin porous carbons by alkaline zinc carbonate and lignin, and combine cobalt nitrate to form Co3O4-LPC catalysts. With 'zero carbon' emissions and low cost.
The photothermal conversion efficiency and catalytic activity of the electrolytic water catalyst are significantly improved, the overpotential of the reaction of hydrogen production by electrolytic water is reduced, the water decomposition reaction is accelerated, and the efficient utilization of solar energy is achieved, and the precious metals is not doped, the cost is low and the environment is friendly.
Smart Images

Figure CN119040935A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of hydrogen production by electrolysis of water, and in particular to a water electrolysis catalyst having both light-heat conversion performance, a preparation method and an application thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Renewable energy represented by solar energy has the contradiction of energy space and time mismatch. Water electrolysis to produce hydrogen and energy storage provides a promising way for the conversion and utilization of solar energy, but the high energy loss and slow reaction kinetics seriously hinder the widespread application of water electrolysis to produce hydrogen. In order to solve this problem, people have invested a lot of energy in developing catalysts to reduce the reaction overpotential and accelerate the water decomposition reaction. Traditional water electrolysis catalysts are mainly precious metals, and the high price of precious metals greatly limits the commercial promotion of water electrolysis to produce hydrogen. In order to solve the problem of high cost of traditional catalysts, people have invested a lot of research on non-precious metals such as iron, cobalt, and nickel. However, the overall energy conversion efficiency of non-precious metal catalysts cannot meet the needs of practical applications. Therefore, new strategies are urgently needed to further improve the electrocatalytic performance of non-precious metal catalysts.
[0004] Carbon materials have the advantages of large specific surface area and high conductivity, which can specifically make up for the shortcomings of non-precious metals that are easy to agglomerate and have poor conductivity. However, in the preparation process of carbon materials such as graphene and carbon nanotubes, fossil fuels are often used as precursors, and the preparation conditions are harsh and the environment is polluted. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a water electrolysis catalyst with both photothermal conversion performance and a preparation method and application, to prepare a porous carbon-loaded non-precious metal water electrolysis catalyst using biomass waste, to improve the water electrolysis catalytic performance using photothermal conversion performance, and to have the advantage of "zero carbon" emissions.
[0006] In order to achieve the above object, the present invention is implemented through the following technical solutions:
[0007] In a first aspect, a method for preparing a water electrolysis catalyst having both light-to-heat conversion performance comprises the following steps:
[0008] S1, mixing and grinding lignin and basic zinc carbonate in a mass ratio of 1: (0.5-1.5), pyrolyzing at 800-1000° C. in an inert atmosphere, and grinding after cooling to obtain a first product;
[0009] S2, washing the first product with acid, rinsing with water until neutral, drying, and grinding to obtain lignin porous carbon LPC;
[0010] S3, adding lignin porous carbon in an amount of 5 to 10 mg / mL to a cobalt nitrate solution with a concentration of 2 to 4 mg / mL, stirring for a set time, drying and grinding to obtain a second product;
[0011] S4, pyrolyzing the second product at 300-400°C, grinding after cooling, and obtaining Co 3 O 4 -LPC powder is a water electrolysis catalyst with both photothermal conversion performance.
[0012] Optionally, in S1, the inert atmosphere is selected from nitrogen, argon or helium, and the gas flow rate is 50 to 100 mL / min.
[0013] Optionally, in S1, the heating rate of the pyrolysis process is 5 to 10°C / min, and the temperature is kept constant for 1 to 3 hours after reaching the set maximum temperature.
[0014] Optionally, in S2, the pickling solution uses hydrochloric acid or sulfuric acid with a concentration of 0.5 to 1.5 mol / L, the mass ratio of the first product to the acid is 1:(15 to 30), and the standing time during the pickling process is 15 to 30 minutes.
[0015] Optionally, in S2, the drying temperature is 80-150° C. and the drying time is more than 10 hours.
[0016] Optionally, in S3, the solvent of the cobalt nitrate solution is water or ethanol.
[0017] Optionally, in S3, the stirring temperature is 20-30°C, and the stirring time is more than 1 hour; the drying temperature is 20-70°C, and the drying time is more than 20 hours.
[0018] Optionally, in S4, pyrolysis is carried out in an air atmosphere with an air flow rate of 30-60 mL / min.
[0019] Optionally, in S4, during the pyrolysis process, the heating rate is 2 to 5°C / min, and after reaching the set maximum temperature, the temperature is kept constant for 0.5 to 1.5 hours.
[0020] Optionally, in S4, grinding is performed to 80-120 mesh.
[0021] In a second aspect, the water electrolysis catalyst having both photothermal conversion performance is prepared by the method for preparing the water electrolysis catalyst having both photothermal conversion performance.
[0022] In a third aspect, the preparation method of the above-mentioned electrolytic water catalyst with photothermal conversion performance and / or the application of the above-mentioned electrolytic water catalyst with photothermal conversion performance in electrolytic water, the electrode used is loaded with the electrolytic water catalyst with photothermal conversion performance; during the electrolysis of water, the electrolytic water catalyst with photothermal conversion performance is exposed to sunlight.
[0023] Optionally, the application includes: application in producing hydrogen by electrolysis of water.
[0024] The beneficial effects of the present invention are as follows:
[0025] 1. The present invention uses basic zinc carbonate as a pore-opening agent and lignin porous carbon LPC prepared from lignin as a matrix, which has a rich pore structure, allowing sunlight to be reflected multiple times in the catalyst pore structure cavity. In addition, the carbon material can absorb most of the sunlight, and can use the lattice thermal vibration caused by the π-π* relaxation effect to efficiently convert solar energy into thermal energy. This makes the catalyst have excellent light-to-heat conversion efficiency, significantly increases the catalyst temperature during the electrolysis of water, and the local high temperature on the surface of the electrocatalyst can promote the thermodynamic and kinetic processes of the electrocatalytic reaction, thereby greatly improving the catalytic activity.
[0026] 2. The present invention can realize the high-value utilization of lignin, a biomass waste, through simple treatment. Biomass has the advantages of abundant reserves and "zero carbon" emissions. It is free of precious metal doping and low cost, which can reduce catalyst costs and improve solar energy utilization, and is of great significance in the development of renewable energy. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0028] Figure 1 The catalyst Co prepared in Example 1 3 O 4 -XRD spectrum of LPC.
[0029] Figure 2 The catalyst Co prepared in Example 1 3 O 4 -LPC SEM images.
[0030] Figure 3 This is an infrared thermal radiation image of an electrode made of the catalyst prepared in Example 1 under AM 1.5G lighting conditions.
[0031] Figure 4 This is the linear sweep voltammetry (LSV) curve of the oxygen evolution reaction (OER) of the catalyst in Example 2.
[0032] Figure 5 This is the linear sweep voltammetry (LSV) curve of the hydrogen evolution reaction (HER) of the catalyst in Example 2.
[0033] Figure 6 This is the linear sweep voltammetry (LSV) curve of the catalyst in Example 2 for the complete water splitting. DETAILED DESCRIPTION
[0034] Example 1
[0035] A method for preparing a water electrolysis catalyst having both light-to-heat conversion performance comprises the following steps:
[0036] S1. Mix lignin and basic zinc carbonate in a mass ratio of 1:1, grind them, put them into an alumina crucible, and place the alumina crucible in a tube furnace. In a nitrogen atmosphere with a flow rate of 80 mL / min, heat the mixture to 900°C at a heating rate of 5°C / min, and then keep the mixture for 2 hours for pyrolysis. After naturally cooling to room temperature, take out the alumina crucible, grind the contents of the crucible, and obtain the first product.
[0037] S2, placing the first product in 1 mol / L hydrochloric acid (the mass ratio of the first product to the hydrochloric acid is 1:20) and letting it stand for 15 minutes, then repeatedly rinsing it with deionized water until it is neutral, and then placing it in a vacuum drying oven at 80°C to fully dry it. After drying, take it out and grind it to 80 mesh to obtain lignin porous carbon LPC;
[0038] S3, dissolving cobalt nitrate hexahydrate in anhydrous ethanol to obtain a cobalt nitrate solution with a concentration of 3 mg / mL, immersing the lignin porous carbon LPC in the prepared cobalt nitrate solution at a ratio of 7.5 mg / mL, stirring for 1 hour at 25°C, then drying in a drying oven at 65°C for 24 hours, and then grinding until the mixture is uniform to obtain a second product;
[0039] S4, the second product was placed in an alumina crucible, the alumina crucible was moved into a tube furnace, and the temperature was increased to 350°C at a rate of 2°C / min in an air atmosphere with a flow rate of 50 mL / min and kept at this temperature for 1 h for pyrolysis, and then naturally cooled to room temperature and taken out, and the contents of the crucible were ground to 80 mesh to obtain the catalyst Co 3 O 4 -LPC is a water electrolysis catalyst with both photothermal conversion performance.
[0040] In the above process, basic zinc carbonate is used as a pore opening agent, mixed with lignin, and pyrolyzed in a nitrogen atmosphere to obtain lignin porous carbon; then acid washing is performed to remove the pyrolysis products of basic zinc carbonate mixed on the lignin porous carbon and impurities such as alkali metals contained in the lignin, and pure lignin porous carbon LPC is obtained as a carrier of a catalyst with a high surface area; the lignin porous carbon LPC is immersed in a cobalt nitrate solution, stirred for a set time to ensure uniform loading, and then dried for 24 hours to ensure sufficient drying; then heat loaded in an oxidizing atmosphere to ensure that the CoO produced by the pyrolysis of cobalt nitrate is completely converted into Co 3 O 4 After grinding to a set fineness, the electrolytic water catalyst Co with sufficient catalytic activity and photothermal conversion capacity is obtained. 3 O 4 -LPC.
[0041] The obtained catalyst Co 3 O 4 -LPC performs XRD test, the results are as follows Figure 1 As shown, characteristic peaks at 31.27°, 36.84°, 44.81°, 59.35°, and 65.23° can be observed, corresponding to Co 3 O 4 The (220)(311)(400)(511) and (440) crystal planes (PDF#43-1003) indicate that the decomposition products of cobalt nitrate are Co 3 O 4 in the form of and was successfully loaded onto the lignin carbon matrix.
[0042] The obtained catalyst Co 3 O 4 -LPC was observed by scanning electron microscope, and the results were as follows Figure 2 As shown, Co 3 O 4 -LPC has a well-developed pore structure, and its average pore size is 6.57nm calculated by BET; this structure can make the Co 3 O 4 The active sites are fully exposed and are conducive to the diffusion of electrolyte ions. On the other hand, under illumination conditions, sunlight can be reflected multiple times in the porous structure cavity to reduce the reflectivity of the catalyst and improve the photothermal conversion effect. The solar spectrum reflectivity instrument measured: the catalyst Co 3 O 4 -The reflectivity of LPC material is as low as 1.1%.
[0043] Example 2
[0044] Based on the catalyst Co prepared in Example 1 3 O 4-Electrodes prepared by LPC and their application in water electrolysis under light conditions.
[0045] The electrode used is loaded with a water electrolysis catalyst having both photothermal conversion performance, and the preparation method of the electrode includes:
[0046] 5 mg of the catalyst Co prepared in Example 1 was added by ultrasonic bath 3 O 4 -LPC material is uniformly dispersed in 1 mL of a mixed solution to prepare a catalyst ink; the mixed solution contains deionized water, isopropanol and Nafion solution.
[0047] The catalyst ink is evenly coated on the carbon cloth and dried to obtain a working electrode loaded with a water electrolysis catalyst with both photothermal conversion performance; the electrode size is 0.5 cm 2 , catalyst Co 3 O 4 -The loading amount of LPC material on carbon cloth is 1mg / cm 2 .
[0048] The photothermal performance test of the obtained working electrode was carried out, specifically: the working electrode was placed under simulated sunlight of AM 1.5G standard at room temperature of 25°C, and the temperature of the working electrode was detected. Figure 3 As shown in the figure, under sunlight irradiation, the electrode temperature can rise to 71.1℃ within 10 minutes, showing good photothermal conversion performance.
[0049] The obtained working electrode was subjected to an electrochemical performance test, which included dark conditions and conditions where the water electrolysis catalyst having both photothermal conversion performance was exposed to sunlight, and the sunlight exposure condition referred to AM 1.5G lighting conditions.
[0050] Including: OER catalytic performance and HER catalytic performance tests, specifically: the obtained working electrode, reference electrode (Hg / HgO electrode) and counter electrode (graphite electrode) are tested in 1M KOH solution using a three-electrode system; during the test, the LSV curve is obtained by linear sweep voltammetry at a scanning rate of 5mV / s, and resistance compensation is performed.
[0051] It also includes: full water splitting performance test, specifically: using the above-mentioned electrodes as cathode and anode at the same time, testing using a double electrode system in 1M KOH solution, obtaining LSV curves by linear scanning voltammetry at a scanning rate of 5mV / s during the test, and performing resistance compensation.
[0052] After the test is completed, the measured potential is converted into the standard hydrogen electrode potential E according to the Nernst equation. RHE , plot the potential as the abscissa:
[0053] E RHE =E Hg / HgO +0.098+0.059×pH;
[0054] In the formula, E RHE refers to the standard hydrogen electrode potential;
[0055] E Hg / HgO It refers to the Hg / HgO electrode potential;
[0056] pH refers to the acidity or alkalinity of the electrolyte;
[0057] 0.098 comes from the technical document "Nano Research, 2024, 17(5): 3769-3776";
[0058] 0.059 comes from the technical document "Nano Research, 2024, 17(5): 3769-3776".
[0059] The test curve of OER catalytic performance is as follows Figure 4 As shown, it can be seen that the catalyst Co 3 O 4 -The OER performance of the working electrode of LPC is greatly improved under light conditions: ① Only 301mV overpotential is required under light conditions to reach 10mA / cm 2 The current density is 43mV lower than that in dark conditions (344mV); ② Under light conditions, only 393mV overpotential is needed to reach 100mA / cm 2 The current density is 93mV lower than that in dark conditions (486mV); ③ The current density can reach 792.6mA / cm under light conditions at 1.8V 2 , much higher than in dark conditions (271.6mA / cm 2 ).
[0060] The test curve of HER catalytic performance is as follows Figure 5 As shown, it can be seen that the catalyst Co 3 O 4 -The HER performance of the working electrode of LPC is greatly improved under light conditions: ① Only 150mV overpotential is required to reach 10mA / cm 2 The current density is 145mV lower than that in dark conditions (295mV); ② Under light conditions, only 328mV overpotential is needed to reach 100mA / cm 2 Current density; ③ Under light conditions, the current density can reach 393.2mA / cm at 0.45V voltage 2 , much higher than in dark conditions (84.4mA / cm 2 ).
[0061] The test curve of the complete water decomposition performance is as follows: Figure 6 As shown, it can be seen that the catalyst Co 3 O 4 -The full water splitting performance of the working electrode of LPC is greatly improved under light conditions: ① Only 371mV overpotential is required under light conditions to reach 10mA / cm 2 The current density is 313mV lower than that in dark conditions (684mV); ② Under light conditions, only 742mV overpotential is needed to reach 100mA / cm 2 The current density is 194mV lower than that in dark conditions (936mV); ③ The current density can reach 594.6mA / cm under light conditions at 2.5V 2 , much higher than in dark conditions (425.4mA / cm 2 ).
[0062] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A method for preparing a water electrolysis catalyst having both light-to-heat conversion performance, characterized in that the steps include: S1, mixing and grinding lignin and basic zinc carbonate in a mass ratio of 1: (0.5-1.5), pyrolyzing at 800-1000° C. in an inert atmosphere, and grinding after cooling to obtain a first product; S2, washing the first product with acid, rinsing with water until neutral, drying, and grinding to obtain lignin porous carbon; S3, adding lignin porous carbon in an amount of 5 to 10 mg / mL to a cobalt nitrate solution with a concentration of 2 to 4 mg / mL, stirring for a set time, drying and grinding to obtain a second product; S4. Pyrolyze the second product at 300-400° C., grind it after cooling, and obtain Co3O4-LPC powder, which is a water electrolysis catalyst with both photothermal conversion performance.
2. The method for preparing a water electrolysis catalyst having both light-to-heat conversion performance according to claim 1, characterized in that: In S1, the inert atmosphere is selected as one of nitrogen, argon or helium, and the gas flow rate is 50-100 mL / min; Optionally, in S1, the heating rate of the pyrolysis process is 5 to 10°C / min, and the temperature is kept constant for 1 to 3 hours after reaching the set maximum temperature.
3. The method for preparing a water electrolysis catalyst having light-to-heat conversion performance according to claim 1, characterized in that: In S2, the pickling solution is hydrochloric acid or sulfuric acid with a concentration of 0.5 to 1.5 mol / L, the mass ratio of the first product to the acid is 1:15 to 1:30, and the standing time during the pickling process is 15 to 30 minutes; Optionally, in S2, the drying temperature is 80-150° C. and the drying time is more than 10 hours.
4. The method for preparing a water electrolysis catalyst having both light-to-heat conversion performance according to claim 1, characterized in that: In S3, the solvent of the cobalt nitrate solution is water or ethanol.
5. The method for preparing a water electrolysis catalyst having both light-to-heat conversion performance according to claim 1, characterized in that: In S3, the stirring temperature is 20-30°C, and the stirring time is more than 1 hour; the drying temperature is 20-70°C, and the drying time is more than 20 hours.
6. The method for preparing a water electrolysis catalyst having both light-to-heat conversion performance according to claim 1, characterized in that: In S4, pyrolysis was carried out in an air atmosphere with an air flow rate of 30–60 mL / min; Optionally, in S4, during the pyrolysis process, the heating rate is 2 to 5°C / min, and after reaching the set maximum temperature, the temperature is kept constant for 0.5 to 1.5 hours.
7. The method for preparing a water electrolysis catalyst having both light-to-heat conversion performance according to claim 1, characterized in that: In S4, grind to 80-120 mesh.
8. A water electrolysis catalyst with both photothermal conversion performance obtained by the preparation method of a water electrolysis catalyst with both photothermal conversion performance as described in any one of claims 1 to 7.
9. A method for preparing a water electrolysis catalyst having both photothermal conversion performance as claimed in any one of claims 1 to 7 and / or use of the water electrolysis catalyst having both photothermal conversion performance as claimed in claim 8 in electrolysis of water, characterized in that: The electrode used is loaded with the water electrolysis catalyst having both photothermal conversion performance; during the water electrolysis process, the water electrolysis catalyst having both photothermal conversion performance is exposed to sunlight.
10. The use according to claim 9, characterized in that The application includes: application in producing hydrogen by electrolysis of water.
Citation Information
Cited By
Method and device for enhancing water electrolysis through photo-thermal coupling
CN121381009A
Graded porous carbon loaded nickel phosphide catalyst and application thereof in benzyl alcohol electrooxidation coupling hydrogen production