Device and method for rapidly preparing hollow nanofibers through airflow induction

The core layer and shell solution are combined in the coaxial needle by airflow induction method, which solves the problems of safety hazards and low production efficiency in electrospinning method, and achieves the rapid, safe and clean preparation of hollow nanofibers with good isolation Thermal and mechanical properties.

CN119041037AActive Publication Date: 2024-11-29SICHUAN UNIV

Patent Information

Application Number
CN202411003648.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-29
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

The existing hollow nanofiber preparation methods have problems such as difficult preparation conditions, low yield, high cost and safety hazards. Especially the electrospinning method has safety hazards and production during spinning of non-conductive precursor solutions under high voltage electric field. Inefficient.

Method used

The core layer and shell solution are combined under high-speed airflow through the coaxial needle by airflow, directly curing to form hollow nanofibers, and the core layer substance is removed by high-temperature calcination, and the design includes coaxial needles for electrospinning and compression. Devices of air pumps, collectors and high temperature calcining devices.

Benefits of technology

It realizes the rapid, safe and clean preparation of a large number of uniform hollow nanofibers, and the fiber diameter is controllable, with good thermal insulation and mechanical properties. It is suitable for the preparation of a variety of materials, improving production efficiency and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119041037A_ABST
    Figure CN119041037A_ABST
Patent Text Reader

Abstract

The invention discloses a device and method for rapidly preparing hollow nanofibers through airflow induction, firstly, the structure of a coaxial needle head is designed, the coaxial needle head is formed by coaxially sleeving two capillary tubes with different inner diameters, and an inner tube at one end of the coaxial needle head extends to the outside of an outer tube to serve as a fiber outlet; the section, close to the fiber outlet end, of the coaxial needle head is bent by 90 degrees to form a vertical section, an airflow pipeline is arranged on the side face of the bent position, and a gas outlet of the airflow pipeline directly faces the vertical section; air flow induction is matched with a coaxial needle head to prepare hollow fibers, a core layer solution and a shell layer solution are injected into the coaxial needle head respectively, the core layer solution and the shell layer solution converge at a fiber outlet and are directly solidified into shell-core coaxial nanofibers under the action of high-speed air flow, and after the fibers are collected through a collector, high-temperature calcination is performed to obtain the shell-core coaxial nanofibers. And removing a nuclear layer substance to obtain the hollow nanofiber. The method disclosed by the invention can be used for rapidly and directly preparing a large number of uniform hollow nanofibers, and is safe and clean.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of material science and engineering technology, and in particular to a device and method for rapidly and massively preparing hollow nanofibers through airflow induction. Background Art

[0002] The one-dimensional nanostructure of polymer materials has the advantages of large aspect ratio, light weight, high temperature resistance, good thermal stability, stable chemical properties and mechanical vibration resistance due to its unique morphological structure, which has a far-reaching impact on many fields such as aerospace, biomedicine, environmental energy, and electronic communications. In order to obtain lighter, more stable, and more flexible one-dimensional nanomaterials, hollow nanofibers have become a new research hotspot. At present, the preparation methods of hollow nanofibers include phase conversion method, template method, extrusion molding method, electrospinning method, etc. However, the above methods may have disadvantages such as difficult preparation conditions, low yield, and high cost, which limit the production and application of hollow nanofibers.

[0003] At present, the preparation method of hollow nanofibers mostly adopts electrospinning, which is basically the same as the principle of traditional preparation of solid fibers, but the device is improved. The spinneret needle is improved on the basis of the traditional electrospinning device. The solutions of core and shell materials are divided into two different syringes, and the spinneret system is composed of two coaxial capillaries with different inner diameters. Under the action of high-voltage electric field, the outer liquid flows out and merges with the core liquid. Since the two solutions merge at the nozzle for a very short time during the spinning process, and the diffusion coefficient of the polymer is low, they will not be mixed together before solidification. Under the action of high-voltage electric field force, the shell liquid is stretched at high frequency and sprayed at high speed. During high-speed spraying, the interface between the inner and outer solutions will produce strong shear stress. Under the action of shear stress, the core solution moves coaxially along the shell, bends, shakes, deforms, and solidifies into ultrafine coaxial composite nanofibers. The coaxial composite nanofibers are treated by solvent extraction or high-temperature calcination to remove the core material, and the physical structure of the outer layer is retained, so as to obtain nanofibers with hollow structure.

[0004] Electrospinning requires high-voltage static electricity to prepare nanofibers. High voltage electricity of 5-30kV will bring many safety hazards. For non-conductive precursor solutions, there is no self-spinning property. Conductive materials are required as collection plates in electrospinning equipment, and some non-conductive surfaces cannot be directly sprayed. The fibers collected by electrospinning are attached to the collection plate, and during the secondary transfer process, they may cause a certain degree of damage to the sample. In the industrial production of electrospinning with multiple needles, there will be mutual influence of electric fields between the overly dense needles, which will interfere with the spinning process and affect the production quality of nanofibers. Therefore, in order to obtain hollow nanofibers with a simple preparation process, high efficiency and large output, it is necessary to develop a direct, fast, efficient and universal method. Summary of the invention

[0005] The object of the present invention is to provide a device and a method for rapidly preparing hollow nanofibers by airflow induction.

[0006] The present invention adopts a method for directly preparing hollow fibers by airflow induction and coaxial needles. A core layer solution and a shell layer solution are respectively injected into coaxial needles formed by two coaxial capillaries with different inner diameters. The two are merged at the fiber outlet of the coaxial needle and directly solidified into shell-core coaxial nanofibers under the action of high-speed airflow. The fibers are collected by a collector; then the core layer material is removed by calcination to obtain hollow nanofibers.

[0007] The invention provides a device for rapidly preparing hollow nanofibers by airflow induction, the structure of which includes: a coaxial needle for electrostatic spinning, a compressed air pump, a collector, a high-temperature calcination device, a shell solution injection pump and a core solution injection pump.

[0008] The coaxial needle is composed of two capillaries with different inner diameters in a coaxial sleeve manner. The inner tube and outer tube ports at one end of the coaxial needle are both sealed, and the inner tube at the other end of the coaxial needle extends to the outside of the outer tube as a fiber outlet. The inner tube is extended by a length H compared to the outer tube, and H is equal to 1 / 2 of the radius of the outer tube. A section of the coaxial needle near the fiber outlet is bent 90° to form a vertical section, and an airflow duct is set on the side of the bend, and the center line of the airflow duct is on the same straight line as the center line of the vertical section. The airflow duct is connected to a compressed air pump, and the gas outlet of the airflow duct is opposite to the vertical section, which is used to apply airflow to the fiber at the fiber outlet. The compressed air pump is used to inject any one of air, nitrogen, argon, and mixed gas into the airflow duct.

[0009] The shell solution injection pump injects the shell solution into the annular space between the inner and outer tubes; the core solution injection pump injects the core solution into the internal cavity of the inner tube; the collector is used to collect the fibers prepared by the coaxial needle; the high-temperature calcination device removes the core layer material through high-temperature sintering to obtain hollow nanofibers.

[0010] Preferably, the collector may be a cage-type collector for collecting the spun fibers to form a three-dimensional structure, which is then calcined to form a hollow nanofiber sponge.

[0011] The device is used for preparing hollow fibers made of any material including polyimide, polyacrylonitrile, yttrium-stabilized zirconia and polyvinyl butyral.

[0012] The present invention also provides a method for rapidly preparing hollow nanofibers by airflow induction, which is achieved by the above-mentioned device. The method steps are as follows:

[0013] S1. Select a shell material and a core solution; the shell material is selected from any one of polyimide, polyacrylonitrile, yttrium-stabilized zirconium oxide, and polyvinyl butyral ester, and a solvent is used to dissolve the shell material to form a shell solution. The selection of the core solution needs to meet the requirements of being incompatible with the shell solution and not reacting, having a viscosity similar to that of the shell material, and being able to be removed by high-temperature calcination during the preparation process. The core solution has no self-spinning requirements and can be two precursor solutions that can be spun, or an oily substance that is non-self-spinning and incompatible.

[0014] S2. The shell solution and the core solution are pushed and injected into the coaxial needle respectively, and gathered at the tip of the coaxial needle. The compressed air pump is turned on to provide airflow. The shell solution and the core solution are stretched under the action of the high-speed airflow to form a coaxial Taylor cone. Then the coaxial jet undergoes a bending unstable motion. At the same time, the solvent evaporates, and the solute is finally solidified and deposited in the collector.

[0015] S3. The collected fibers are calcined at high temperature to remove the core layer material to obtain hollow nanofibers.

[0016] Preferably, polyethylene oxide PEO or polyvinyl pyrrolidone PVP may be added to the shell layer solution to increase the viscosity and spinnability of the solution.

[0017] Preferably, in step S2, the propulsion rate ratio of the shell layer solution and the core layer solution in the coaxial needle is controlled to be 2:1.

[0018] Compared with the prior art, the present invention is beneficial in that:

[0019] (1) The method of the present invention can rapidly and directly prepare a large number of uniform hollow nanofibers in a safe and clean manner; the prepared hollow nanofibers have controllable diameters and good uniformity, and the prepared materials have good applications in the fields of thermal insulation, mechanical high-temperature elasticity, etc.

[0020] (2) The device and method of the present invention prepare hollow fiber structures at the physical level through the design of coaxial needles. All systems with self-spinning properties (polymers, ceramics, etc.) are applicable, and this preparation method has good portability.

[0021] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 : Schematic diagram of the structure of the device for rapidly preparing hollow nanofibers by airflow induction provided by the present invention.

[0023] Figure 2: Structural diagram of the coaxial needle. (a) shows the relationship between the airflow direction and the position of the coaxial needle, and (b) shows the specific dimensions of the coaxial needle in this embodiment.

[0024] Figure 3 : Optical photographs of the formation, stretching process and shell-core structure of the coaxial jet under a high-speed camera.

[0025] Figure 4 :Different V in / V out The SEM images of the fibers obtained under the ratio of V in / V out =1 / 4, (b) is the SEM image of the beaded fibers obtained, and (c) is the SEM image of the V in / V out =1 / 2. SEM image of uniform hollow fiber obtained.

[0026] Figure 5 : Performance diagram of sponge made of polyimide hollow nanofibers; (a) is an ultra-light demonstration diagram, (b) is a low-magnification SEM image of polyimide hollow nanofibers, (c) is a high-magnification SEM image, and (d) is a fiber diameter distribution diagram.

[0027] Figure 6 : Thermal conductivity performance diagram of polyimide hollow nanofiber sponge; (a) is the relationship between thermal conductivity and sponge density, and (b) is a comparison diagram of the working space of polyimide hollow nanofiber sponge and other thermal insulation sponges.

[0028] Figure 7 : Test results of heat resistance of polyimide hollow nanofiber sponge and other materials; (a) is a comparison of thermogravimetric curves of polyimide hollow nanofiber sponge, polyurethane sponge, polystyrene sponge and cork, (b) is a curve of surface temperature and time of samples in heat resistance comparison experiment of polyimide hollow nanofiber sponge, polyurethane sponge and polystyrene sponge, (c) is a comparison of optical and infrared thermal imaging of heat resistance comparison experiment.

[0029] Figure 8 : Infrared thermal imaging of polyimide hollow nanofiber sponge.

[0030] Fig. 9 : Demonstration diagram of compression and recovery of polyimide hollow nanofiber sponge at different temperatures.

[0031] Fig.10 : Fatigue test curves of hollow nanofiber sponges with different densities; (a) is the density of 50 mg / cm 3 1000 times fatigue test curve of hollow nanofiber sponge, (b) is the density of 80mg / cm 3Fatigue test curve of fiber sponge with strain of 80% for 1000 times.

[0032] Fig.11 : Optical image of the hollow nanofiber sponge recovered after 180° bending and folding.

[0033] Fig.12 : Polyimide hollow nanofiber sponges in various colors.

[0034] Fig.13 : Comparative experiment of hollow nanofiber sponge filled with argon and air after evacuation. DETAILED DESCRIPTION

[0035] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0036] like Figure 1 As shown, the structure of the device for rapidly preparing hollow nanofibers by airflow induction provided by the present invention includes a coaxial needle for electrospinning, a compressed air pump, a collector, a high-temperature calcination device, a shell solution injection pump and a core solution injection pump.

[0037] The coaxial needle is designed as follows: Figure 2 As shown in FIG. 1 , the coaxial needle is composed of two capillaries with different inner diameters in a coaxial sleeve arrangement. The inner tube and outer tube ports at one end of the coaxial needle are both sealed, and the inner tube at the other end of the coaxial needle extends to the outside of the outer tube as the fiber outlet. The inner tube is extended by a length H compared to the outer tube. A section of the coaxial needle near the fiber outlet is bent 90° to form a vertical section. An airflow duct is set on the side of the bend, and the center line of the airflow duct is on the same straight line as the center line of the vertical section (see FIG. 1 ). Figure 2 a). The air flow pipeline is connected to a compressed air pump, and the gas outlet of the air flow pipeline is opposite to the vertical section, which is used to apply air flow to the fiber at the fiber outlet. The compressed air pump is used to inject any one of air, nitrogen, argon, and mixed gas into the air flow pipeline. In practical applications, the wall thickness of the hollow fiber obtained after calcination can be adjusted by changing the ratio of the inner diameter of the inner tube and the outer tube of the coaxial needle. The value of H will directly affect the structural formation of the hollow fiber. If H is too small, the core layer solution in the inner tube will be blocked by the shell layer solution in the outer tube. At this time, the core layer solution cannot be stretched, and the shell layer solution forms a jet alone. Figure 3 As shown in the figure, when H is increased to 1 / 2 of the outer tube radius, a better coaxial jet can be obtained. At this time, the Taylor cone part becomes significantly longer and can be clearly observed. Figure 3The formation process and coaxial jet captured by a high-speed camera are shown (the core material is the red part, and the shell material is the transparent part); when H is further increased to be greater than the radius of the outer tube, the shell solution flows out along the outer surface of the inner tube and cannot completely cover the core solution in the inner tube, and a stable single coaxial jet cannot be obtained. Therefore, in the present invention, H is set equal to 1 / 2 of the radius of the outer tube. Figure 3 It is also explained that the coaxial jet of the device of the present invention is stable and uniform without splitting or droplets.

[0038] The shell solution injection pump injects the shell solution into the annular space between the inner and outer tubes. The core solution injection pump injects the core solution into the inner cavity of the inner tube. The collector is used to collect the fibers prepared by the coaxial needle, preferably a cage-type collector, which is used to collect the spun fibers to form a three-dimensional structure. The high-temperature calcination device removes the core layer material by high-temperature sintering to obtain hollow nanofibers.

[0039] The device for rapidly preparing hollow nanofibers by airflow induction of the present invention has a simple structure and a simple spinning process. In industrial production, multiple needles can be spun simultaneously, and the production efficiency is high.

[0040] The above device is used to prepare polyimide hollow fibers, and the specific method is as follows:

[0041] First, prepare the shell solution A: use an electronic balance to weigh 0.8g of polyethylene oxide (PEO) powder and add it to 10g of N,N-dimethylformamide (DMF) solution, and stir it magnetically at 60°C for 3 hours until it is completely dissolved. Then, add 10g of polyacrylic acid (PAA)-DMF solution (20wt.%) to the previously prepared PEO solution, and continue to stir it magnetically at 50°C for 6 hours until a uniform polyacrylic acid (PAA) precursor solution is obtained, which is the shell solution A.

[0042] Preparation of core layer solution B: Dimethyl silicone oil (PMX-200, 12500 cSt) was used as the core layer material and heated to 60°C under magnetic stirring.

[0043] The polyacrylic acid (PAA) precursor solution and dimethyl silicone oil were respectively introduced into the coaxial needle as the shell solution and the core solution while hot; the flow rate of the outer axis solution was 0.02 mL min -1 The flow rate of the inner axis solution is 0.01 mL min -1, the air flow velocity remains stable at 0.1Mpa. Under the shear force of the high-speed airflow, the shell-core solution converges and stretches at the needle tip to form a Taylor cone, and then the coaxial jet undergoes a bending unstable motion. At the same time, the solvent evaporates, and the solute is finally solidified and deposited on the collection device to form a polyacrylic acid-dimethyl silicone oil coaxial nanofiber sponge. The collected coaxial nanofiber spinning precursor sponge was kept at 70℃ in a vacuum oven for 8 hours to evaporate all the residual DMF solution during the spinning process. Then it was heated to 320℃ in a muffle furnace at 2.6℃ / min and kept for 120min, and cooled with the furnace. Since polyacrylic acid (PAA) undergoes thermal imidization to form polyimide, dimethyl silicone oil will be thermally decomposed at 320℃ into products such as silane and carbon dioxide, which will evaporate, and finally a three-dimensional structure composed of polyimide hollow nanofibers is obtained.

[0044] In the above method, the shell-core solution advancing rate ratio has a great influence on the formation of the hollow structure. in / V out =1 / 4, the morphology of the fiber after calcination found that the fiber was porous and did not obtain an ideal hollow structure. The flow rate of methyl silicone oil was small and its continuous filamentation performance was poor. At this time, the methyl silicone oil was distributed in the original silk in the form of droplets, forming a beaded fiber structure, such as Figure 4 (a). When V in / V out = 1 / 2, the morphology of the calcined fiber can be found to have an obvious hollow structure, which increases the flow rate of the core liquid. At this time, the interfacial shear stress is sufficient to make the methyl silicone oil continuously distributed inside the fiber, such as Figure 4 (b). Then continue to increase the flow rate ratio V in / V out When it is larger than 1 / 2, the PI solution cannot cover the methyl silicone oil, and a coaxial jet cannot be obtained at the needle tip. The methyl silicone oil drips in the form of droplets. Only the PI solution forms a jet.

[0045] Figure 5 It is a sponge composed of polyimide hollow nanofibers and its ultra-light demonstration (a) low-magnification SEM image of polyimide hollow nanofibers (b), high-magnification SEM image (c), and fiber diameter distribution image (d). As can be seen from the figure, the present invention can obtain ultra-light hollow nanofibers and sponge structures, and can easily produce a large number of hollow nanofiber sponge structures with uniform fiber diameters and a large number of high-quality hollow structures.

[0046] Figure 6The figure is a graph showing the relationship between the thermal conductivity of the polyimide hollow nanofiber sponge and the sponge density (a), and a comparison of the working space of the polyimide hollow nanofiber sponge and other thermal insulation sponges (b). As can be seen from the figure, the hollow nanofiber sponge prepared by the present invention has low thermal conductivity and its density can be controlled. At the same density, its thermal conductivity is lower than that of other polymer thermal insulation sponges, reflecting the advantages of hollow nanofibers.

[0047] Figure 7 The thermogravimetric curves of polyimide hollow nanofiber sponge, polyurethane sponge, polystyrene sponge and cork (a), the curves of the surface temperature and time of the samples in the heat resistance comparison experiment of polyimide hollow nanofiber sponge, polyurethane sponge and polystyrene sponge (b), and the comparison of optical and infrared thermal imaging of the heat resistance comparison experiment (c). As can be seen from the figure, compared with the existing finished thermal insulation materials (polystyrene sponge PS, polyurethane sponge PU, cork), the maximum working temperature of polyimide hollow nanofiber sponge can reach 400℃, and its thermal insulation performance is excellent.

[0048] Figure 8 This is an infrared thermal image of a polyimide hollow nanofiber sponge heated on a 400°C hot stage for 120 minutes. As can be seen from the image, the polyimide hollow nanofiber sponge can work for a long time at 400°C and has good thermal stability.

[0049] Fig. 9 This is a demonstration diagram of the compression and recovery of polyimide hollow nanofiber sponge at different temperatures. Fig.10 (a) and (b) are respectively the density of 50 mg / cm 3 The fatigue test curve of hollow nanofiber sponge with a density of 80 mg / cm 3 Fatigue test curve of fiber sponge with strain of 80% for 1000 times. Fig.11 This is an optical image of the hollow nanofiber sponge after being bent and folded at 180°. As can be seen from the figure, the hollow nanofiber sponge prepared by the present invention has good elasticity at both high and low temperatures (-196°C to 300°C), and the hollow nanofiber sponge can withstand 1000 cycles of 80% strain compression tests and has good fatigue resistance.

[0050] Fig.12 The polyimide hollow nanofiber sponge with various colors can be obtained by dyeing the core layer solution. The polyimide hollow nanofiber sponge with various colors can be obtained by filling the core layer with solutions of different colors.

[0051] Fig.13The hollow nanofiber sponge is evacuated and then fully filled with argon in an argon atmosphere. Then the same sample is filled with argon and air respectively and allowed to fall freely from the same height. Because argon is lighter than air, the sample filled with argon falls more slowly than the sample filled with air. It can be seen that there are a large number of entangled and complex hollow tube structures in the polyimide hollow nanofiber sponge, which can be filled and adsorbed with gas and will not be completely exchanged with the air in a short time. From the picture of the same frame of the high-speed camera, it can be seen that the free fall speed of the sample filled with argon is significantly slower than that of the sample filled with air. If there is a better packaging process in the future, practical applications such as gas storage can be realized.

[0052] In summary, the preparation method of the present invention is efficient and clean and is suitable for industrial production. The prepared hollow fiber can realize color diversity, gas storage, adsorption and other additional functions in addition to the basic functions of flexibility, elasticity, and thermal insulation.

[0053] The above description is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present invention. Although the present invention has been disclosed as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A device for rapidly preparing hollow nanofibers by airflow induction, It is characterized in that It includes a coaxial needle for electrospinning, a compressed air pump, a collector, a high-temperature calcination device, a shell solution injection pump and a core solution injection pump; The coaxial needle is composed of two capillaries with different inner diameters in a coaxial sleeve manner, the inner tube and outer tube ports at one end of the coaxial needle are both sealed, and the inner tube at the other end of the coaxial needle extends to the outside of the outer tube as a fiber outlet, and the inner tube extends out of the outer tube by a length H, which is equal to 1 / 2 of the radius of the outer tube; a section of the coaxial needle near the fiber outlet is bent 90° to form a vertical section, and an airflow duct is arranged on the side of the bend, and the center line of the airflow duct is on the same straight line as the center line of the vertical section; the airflow duct is connected to a compressed air pump, and the gas outlet of the airflow duct faces the vertical section, so as to apply airflow to the fiber at the fiber outlet; The shell solution injection pump injects the shell solution into the annular space between the inner and outer tubes; The core layer solution injection pump injects the core layer solution into the inner cavity of the inner tube; the collector is used to collect the fibers prepared by the coaxial needle; the high-temperature calcination device removes the core layer material through high-temperature sintering to obtain hollow nanofibers.

2. The device for rapidly preparing hollow nanofibers by airflow induction as claimed in claim 1, It is characterized in that The compressed air pump is used to inject any one of air, nitrogen, argon and mixed gas into the air flow pipeline.

3. The device for rapidly preparing hollow nanofibers by airflow induction as claimed in claim 1, It is characterized in that The device is used for preparing hollow fibers made of any material including polyimide, polyacrylonitrile, yttrium-stabilized zirconia and polyvinyl butyral.

4. The device for rapidly preparing hollow nanofibers by airflow induction as claimed in claim 1, It is characterized in that The collector is a cage-type collector, which is used to collect spun fibers to form a three-dimensional structure.

5. A method for rapidly preparing hollow nanofibers by airflow induction, It is characterized in that Use the device as described in any one of claims 1-4.

6. The method for rapidly preparing hollow nanofibers by airflow induction as claimed in claim 5, It is characterized in that Here are the steps: S1, selecting a shell material and a core solution; the shell material is selected from any one of polyimide, polyacrylonitrile, yttrium-stabilized zirconium oxide, and polyvinyl butyral ester, and a solvent is used to dissolve the shell material to form a shell solution; the core solution needs to be incompatible with and non-reactive with the shell solution, have a viscosity similar to that of the shell material, and can be removed by high-temperature calcination during the preparation process; S2, respectively push the shell solution and the core solution into the coaxial needle and gather them at the tip of the coaxial needle. Turn on the compressed air pump to provide airflow. The shell solution and the core solution are stretched under the action of the high-speed airflow to form a coaxial Taylor cone. Then the coaxial jet undergoes bending and unstable motion. At the same time, the solvent evaporates and the solute is finally solidified and deposited in the collector. S3. The collected fibers are calcined at high temperature to remove the core layer material to obtain hollow nanofibers.

7. The method for rapidly preparing hollow nanofibers by airflow induction as claimed in claim 6, It is characterized in that Polyethylene oxide PEO or polyvinyl pyrrolidone PVP is also added to the shell layer solution to increase the viscosity and spinnability of the solution.

8. The method for rapidly preparing hollow nanofibers by airflow induction as claimed in claim 6, It is characterized in that In step S2, the propulsion rate ratio of the shell layer solution and the core layer solution in the coaxial needle is controlled to be 2:1.

Citation Information

Patent Citations

  • Preparation method of hollow fiber in coaxial electrostatic spinning

    CN103088442A

  • Nano material preparation device

    CN108950701A

  • Method for preparing para-aramid nanofiber membrane through airflow-assisted drafting coaxial spinning

    CN117344457A

  • Thermal insulation material, and preparation method therefor and use thereof

    WO2023040966A1

Cited By

  • Method for preparing high-crimpness superfine fibers under action of high-speed airflow and core-shell

    CN120006414A

  • Method for preparing high-curling ultrafine fibers by high-speed airflow and core-shell interaction

    CN120006414B