Method for measuring embossing depth

By scanning the embossing depth of battery electrodes with a two-dimensional microscope, the problem of inaccurate embossing depth measurement in existing technologies has been solved, enabling precise control of embossing depth and improving battery production quality and safety.

CN119043207APending Publication Date: 2024-11-29JIANGXI ANCHI NEW ENERGY TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411165620.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing methods for measuring the embossing depth of battery electrodes have significant errors, leading to embossing deformation and inaccurate measurement results, which affect the manufacturing quality and performance of batteries.

Method used

A two-dimensional microscope is used to scan the embossing depth. The average embossing depth is calculated by measuring the depth difference from the center point to the edge of the embossing. The process parameters are then adjusted to ensure that the embossing depth is within the standard range.

Benefits of technology

It provides more realistic and accurate embossing depth measurement results, reduces defect rate, avoids lithium plating, and improves battery performance and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119043207A_ABST
    Figure CN119043207A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of measurement, particularly relates to a method for measuring the embossing depth, and aims at solving the problems that an existing measurement method has large errors and causes embossing deformation. The method comprises the following steps: (a) preparing a quadratic element microscope with a depth scanning function; (b) placing the embossed pole piece on a workbench of a microscope; (c) performing deep scanning on the embossing indentation on the pole piece by using a microscope to obtain three-dimensional image information; (d) determining the position of a central point of the embossing; (e) selecting at least one reference point; (f) measuring the depth difference between the reference point and the central point; (g) calculating the average depth of embossing; (h) analyzing the average depth data to evaluate whether the embossing is too deep; (i) if the embossing is too deep, adjusting the process parameters until a predetermined criterion is met. According to the method, a more accurate measurement result can be provided, the lithium precipitation phenomenon is effectively avoided, and the battery manufacturing quality and safety are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of measurement technology, and in particular relates to a method for measuring embossing depth. Background Art

[0002] In the battery manufacturing process, in order to ensure the consistency and safety of battery performance, the embossing on the battery pole piece needs to be accurately measured. During the embossing process, if the embossing is too deep, it may cause lithium precipitation, which will not only affect the capacity and cycle life of the battery, but also may cause safety problems. Therefore, it is crucial to develop a method that can accurately measure the embossing depth.

[0003] The existing measurement method is usually to use a micrometer to directly measure the thickness of the electrode after embossing. However, this method has a large measurement error and may cause deformation of the embossing, resulting in a significant difference between the measured result and the actual value. This inaccurate measurement result will directly affect the manufacturing quality of the battery and the performance of the final product. Summary of the invention

[0004] The purpose of the present invention is to provide a method for measuring embossing depth, accurately measuring the embossing depth on a battery electrode, avoiding lithium deposition caused by excessive embossing, and solving the problems in the prior art mentioned in the above background technology.

[0005] To achieve the above object, the present invention adopts the following technical solution: A method for measuring embossing depth comprises the following steps:

[0006] a) prepare a two-dimensional microscope with a depth scanning function; b) place the electrode with embossing to be tested on the workbench of the two-dimensional microscope; c) use the microscope to perform a depth scan on the embossed indentation on the electrode to obtain three-dimensional image information of the indentation; d) determine the center point position of the embossing in the three-dimensional image information; e) select at least one reference point from the center point to the edge of the indentation; f) use the microscope to measure the depth difference between the reference point and the center point; g) calculate the average depth of the embossing based on the depth difference; h) analyze the average depth data to evaluate whether the embossing is too deep; i) if the analysis result shows that the embossing is too deep, adjust the embossing process parameters until the predetermined standard is met.

[0007] Preferably, in step a), it also includes: a1) adjusting the illumination brightness of the microscope to ensure that the indentation outline is clearly visible; a2) setting the focal length of the microscope under lighting conditions to obtain the best focusing effect of the indentation; a3) calibrating the depth scanning range of the microscope according to the focal length setting; a4) starting the depth scanning function of the microscope and starting the depth scanning of the indentation according to the calibration result in step a3).

[0008] Preferably, in step b), it also includes: b1) cleaning the surface of the pole piece to remove impurities that affect the depth measurement accuracy; b2) placing the cleaned pole piece flat on the workbench of the microscope and ensuring that the embossed surface faces upward; b3) adjusting the position of the pole piece in step b2) so that its embossing is located in the center of the observation field of the microscope; b4) fixing the pole piece in step b2) to prevent movement during the depth scanning process.

[0009] Preferably, in step c), it also includes: c1) adjusting the focus of the microscope to the embossed surface of the pole piece; c2) setting the scanning parameters of the microscope to adapt to the indentation characteristics on the pole piece; c3) performing the depth scan to obtain three-dimensional image information of the indentation on the pole piece; c4) recording the three-dimensional image information in step c3) for subsequent analysis and processing.

[0010] Preferably, in step d), it also includes: d1) selecting an embossed area in the three-dimensional image information; d2) identifying the highest point in the embossed area in step d1) as the center point of the embossing; d3) marking the position coordinates of the center point in step d2) as a reference point for subsequent measurements; d4) recording the position coordinate information of the center point in step d3).

[0011] Preferably, in step e), it also includes: e1) finding different directions around the center point in the three-dimensional image information; e2) selecting at least one direction from the different directions as the direction of the reference point; e3) finding the position of the indentation edge outward from the center point in step d) along the direction in step e2); e4) marking the edge position in step e3) as a reference point and recording its coordinate information.

[0012] Preferably, in step f), it also includes: f1) using the microscope to align the position of the reference point in step e); f2) measuring the vertical distance between the reference point in step f1) and the center point in step d); f3) determining the depth difference of the reference point relative to the center point based on the vertical distance in step f2); f4) recording the depth difference value in step f3).

[0013] Preferably, in step g), it also includes: g1) collecting the depth difference values ​​between each reference point and the center point in step f); g2) adding the depth difference values ​​in step g1) to obtain a total; g3) calculating the total number of the depth difference values ​​in step g1); g4) obtaining the average depth of embossing by dividing the total in step g2) by the number in step g3).

[0014] Preferably, in step h), it also includes: h1) comparing the average depth data in step g) with a preset standard depth threshold; h2) if the average depth in step h1) exceeds the standard depth threshold, judging that the embossing is too deep; h3) recording the judgment result in step h2); h4) taking corresponding process adjustment measures based on the recorded result in step h3).

[0015] Preferably, step i) also includes: i1) adjusting the embossing process parameters according to the analysis result in step h) if the embossing is too deep; i2) re-executing steps b) to h) to verify the adjusted process parameters; i3) comparing the verification result in step i2) with a predetermined standard; i4) if the verification result in step i3) does not meet the predetermined standard, repeating steps i1) to i3) until the predetermined standard is met.

[0016] Technical effects and advantages of the present invention: Compared with the prior art, the method for measuring embossing depth proposed by the present invention has the following advantages:

[0017] The present invention proposes to use a two-dimensional microscope to measure the embossing depth, by performing a depth scan on the embossing indentation and calculating the depth difference from the embossing center point to the edge to reflect the actual indentation depth. This method can provide more realistic and accurate measurement results, help improve production quality and reduce defective product rates. By accurately controlling the embossing depth, the occurrence of lithium plating can be effectively avoided, thereby improving the overall performance and safety of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 Flow chart of the method for measuring embossing depth according to the present invention. DETAILED DESCRIPTION

[0019] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0020] The present invention provides a method for measuring embossing depth, such as Figure 1 As shown, the following steps are included:

[0021] a) preparing a two-dimensional microscope having a depth scanning function to ensure that it can provide high-resolution three-dimensional image information; further comprising:

[0022] Adjust the microscope illumination brightness

[0023] a1) Adjust the illumination brightness of the microscope to ensure that the indentation outline is clearly visible. For example, the light source intensity can be gradually increased or decreased until the indentation outline becomes clear enough for subsequent depth scanning.

[0024] Setting the focus of the microscope

[0025] a2) Under the adjusted lighting conditions, set the focus of the microscope to ensure that the indentation can obtain the best focus effect. The focus of the microscope can be adjusted manually or automatically until the indentation is completely and clearly presented in the field of view.

[0026] Calibrating the depth scanning range of a microscope

[0027] a3) Calibrate the depth scan range of the microscope according to the focal length set in step a2). Ensure that the depth scan covers the entire indentation area and can accurately capture the depth information of the indentation by moving the microscope stage or adjusting the position of the lens.

[0028] Activate the Deep Scan feature

[0029] a4) Start the depth scan function of the microscope and start the depth scan of the indentation according to the calibration result in step a3). Make sure the microscope is stable during the scanning process to avoid any factors that may affect the measurement accuracy.

[0030] Through the above steps, it can be ensured that the two-dimensional microscope can provide accurate and clear image information when measuring the embossing depth, thereby ensuring the accuracy of subsequent measurements. These steps are key components for achieving precise measurements and help improve the reliability and efficiency of overall measurements.

[0031] b) placing the electrode with embossing to be tested on the workbench of the two-dimensional microscope; further comprising:

[0032] Clean the electrode surface

[0033] b1) Use appropriate cleaning agents and tools to clean the surface of the electrode to remove impurities that may affect the depth measurement accuracy. For example, you can use a dust-free cloth dipped in isopropyl alcohol to gently wipe the surface of the electrode to ensure that the surface is clean and dust-free.

[0034] Place the pole piece

[0035] b2) Place the cleaned electrode flat on the microscope workbench, with the embossed surface facing upwards. This ensures that the indentation is clearly visible, facilitating subsequent depth scanning.

[0036] Adjust the pole piece position

[0037] b3) adjusting the position of the electrode in step b2) so that the embossing is located in the center of the observation field of the microscope. The position of the workbench can be adjusted manually or automatically to ensure that the embossing is exactly in the center of the microscope field of view for subsequent depth measurement.

[0038] Fixed pole piece

[0039] b4) Fix the pole piece in step b2) to prevent it from moving during the depth scan. You can use the clamp that comes with the microscope or a specially designed fixture to fix the pole piece to ensure that the pole piece remains stationary during the depth scan.

[0040] The above steps can ensure that the electrode to be tested is in the best position during the measurement process, thereby improving the accuracy of the measurement. These steps are crucial to achieve accurate embossing depth measurement and help improve the reliability and efficiency of the overall measurement.

[0041] c) using the microscope to perform a depth scan on the embossed indentation on the pole piece to obtain three-dimensional image information of the indentation; further comprising:

[0042] Adjust the focus of the microscope

[0043] c1) Adjust the focus of the microscope to the embossed surface of the electrode to ensure that the indentation outline is clearly visible. The focus can be adjusted manually or automatically until the indentation details are clearly visible.

[0044] Set up the scanning parameters of the microscope

[0045] c2) Setting the scanning parameters of the microscope to adapt to the indentation characteristics on the electrode piece. For example, the scanning speed, resolution and other parameters can be adjusted according to the size and depth of the indentation to obtain the best scanning effect.

[0046] Perform a Deep Scan

[0047] c3) performing the depth scan to obtain the three-dimensional image information of the indentation on the pole piece. Ensure that the microscope is stable during the scanning process to avoid any factors that may affect the measurement accuracy.

[0048] Recording 3D image information

[0049] c4) recording the three-dimensional image information in step c3) for subsequent analysis and processing, which can be stored in a data storage system provided by the microscope or connected to a computer for subsequent analysis and processing.

[0050] Through the above steps, it can be ensured that the two-dimensional microscope can provide accurate and clear image information when measuring the embossing depth, thereby ensuring the accuracy of subsequent measurements. These steps are key components for achieving precise measurements and help improve the reliability and efficiency of overall measurements.

[0051] d) determining the center point position of the embossing in the three-dimensional image information; further comprising:

[0052] Select embossing area

[0053] d1) Selecting an embossed area in the three-dimensional image information. The embossed area can be determined by manual selection or automatic software recognition to ensure that only the embossed area is focused on and other irrelevant areas are not included.

[0054] Identify the center point of the embossing

[0055] d2) Identify the highest point in the embossing area in step d1) as the center point of the embossing. Usually, the highest point of the embossing is the center point, and the software tool provided by the microscope or professional image processing software can be used to automatically identify the highest point.

[0056] Mark the center point

[0057] d3) Mark the position coordinates of the center point in step d2) as a reference point for subsequent measurements. The exact position of the center point can be marked on the microscope software interface for quick positioning in subsequent operations.

[0058] Record the center point coordinates

[0059] d4) Record the position coordinate information of the center point in step d3). These coordinate information will be recorded for depth measurement and analysis in subsequent steps.

[0060] Through the above steps, it is possible to ensure that the center point of the embossing is accurately determined in the 3D image information, which is the basis for subsequent depth measurement. These steps help to improve the accuracy and reliability of the measurement and provide accurate data support for subsequent depth analysis.

[0061] e) selecting at least one reference point from the center point to the edge of the indentation; further comprising:

[0062] Find different directions around a center point

[0063] e1) Finding different directions around the center point in the three-dimensional image information. The directions around the center point can be identified manually or automatically using tools on the microscope software interface.

[0064] Select the direction of the reference point

[0065] e2) selecting at least one direction from the different directions as the direction of the reference point. Multiple directions may be selected to ensure full coverage of the indentation edge and improve measurement accuracy.

[0066] Find the location of the indentation edge

[0067] e3) Find the position of the edge of the indentation from the center point of step d) along the direction described in step e2). The edge position can be manually tracked or automatically detected using tools provided by the microscope software to ensure that the selected reference point falls accurately on the edge of the indentation.

[0068] Mark and record reference points

[0069] e4) Mark the edge position described in step e3) as a reference point and record its coordinate information. Mark the exact position of each reference point on the microscope software interface and record these coordinate information for subsequent depth measurement.

[0070] Through the above steps, it is possible to ensure that appropriate reference points are selected from the center point to the edge of the indentation, and the position coordinates of these reference points are accurately marked. These steps help improve the accuracy of subsequent depth measurements and ensure the authenticity and reliability of the measurement results.

[0071] f) measuring the depth difference between the reference point and the center point using the microscope; further comprising:

[0072] Alignment reference point position

[0073] f1) Using the microscope to align the positions of the reference points in step e) Ensure that the focus of the microscope is accurately aligned with each selected reference point to facilitate accurate measurement.

[0074] Measuring vertical distance

[0075] f2) Measure the vertical distance between the reference point in step f1) and the center point in step d). This measurement can be performed using the built-in measurement tool of the microscope to ensure the accuracy of the measurement.

[0076] Determining Depth Difference

[0077] f3) Determine the depth difference of the reference point relative to the center point according to the vertical distance in step f2). The depth difference of the indentation is obtained by calculating the vertical distance difference between the center point and the reference point.

[0078] Record depth difference value

[0079] f4) Recording the depth difference value in step f3). Record the measured depth difference value for subsequent calculation and analysis.

[0080] Through the above steps, it can be ensured that the depth difference between the reference point and the center point is accurately measured using the two-dimensional microscope, which is an important basis for calculating the average embossing depth.

[0081] g) calculating the average depth of embossing according to the depth difference; further comprising:

[0082] Collect depth difference values

[0083] g1) Collect the depth difference values ​​between each reference point and the center point as described in step f). Ensure that all selected reference points are taken into account in order to calculate an overall average depth.

[0084] Calculate the sum of depth differences

[0085] g2) Adding the depth difference values ​​in step g1) to obtain a total. Adding all the collected depth difference values ​​to obtain a total depth difference value.

[0086] Calculate the total number of depth difference values

[0087] g3) Calculating the total number of the depth difference values ​​in step g1) and counting the number of the collected depth difference values ​​to determine the number of samples used to calculate the average depth.

[0088] Calculate average depth

[0089] g4) The average depth of the embossing is calculated by dividing the sum in step g2) by the number in step g3). The average depth of the embossing is calculated by dividing the sum by the total number.

[0090] The above steps ensure that the average embossing depth is accurately calculated, which is a key indicator for evaluating whether the embossing is too deep. These steps help improve the accuracy and reliability of the measurement results, ensuring that subsequent analysis and decision-making are based on reliable data.

[0091] h) analyzing the average depth data to assess whether the embossing is too deep; further comprising:

[0092] Comparing average depth data to standard depth thresholds

[0093] h1) Comparing the average depth data in step g) with a preset standard depth threshold. Comparing the calculated average depth data according to industry standards or standard depth thresholds set within the enterprise.

[0094] Determine whether the embossing is too deep

[0095] h2) If the average depth in step h1) exceeds the standard depth threshold, it is judged that the embossing is too deep. If the average depth exceeds the set threshold, it means that the embossing depth exceeds the allowable range.

[0096] Record the judgment results

[0097] h3) Record the judgment result in step h2). Record the judgment result as a basis for subsequent adjustment of process parameters.

[0098] Take appropriate process adjustment measures

[0099] h4) taking corresponding process adjustment measures based on the recorded results in step h3). If the embossing is too deep, the embossing process parameters need to be adjusted according to the recorded results to ensure that the embossing depth is within the specified range.

[0100] Through the above steps, it can be ensured that whether the embossing depth is too deep is accurately evaluated, and reasonable process adjustments can be made accordingly to improve product quality and production efficiency.

[0101] i) if the analysis result shows that the embossing is too deep, adjusting the embossing process parameters until the predetermined standard is met; further comprising:

[0102] Adjust process parameters based on analysis results

[0103] i 1) According to the analysis result in step h), if the embossing is too deep, the embossing process parameters are adjusted, which may include adjusting the pressure, the design of the embossing die, the embossing speed and other factors to reduce the embossing depth.

[0104] Repeat the measurement procedure

[0105] i2) Re-execute steps b) to h) to verify the adjusted process parameters. This means that the sample needs to be re-prepared and the entire measurement process repeated to ensure that the adjusted process parameters do produce the expected effect.

[0106] Compare validation results with pre-determined standards

[0107] i 3) Comparing the verification result in step i 2) with a predetermined standard. Checking whether the new measurement result meets the predetermined embossing depth standard.

[0108] Repeat the adjustment process until the target is reached.

[0109] i4) If the verification result in step i3) does not meet the predetermined standard, repeat steps i1) to i3) until the predetermined standard is met. If the new measurement result still does not meet the standard, it is necessary to continue to adjust the process parameters and re-measure until the predetermined standard is met.

[0110] Through the above steps, it can be ensured that after the embossing process parameters are properly adjusted, the embossing depth can meet the predetermined standards, thereby avoiding the occurrence of lithium plating and improving the quality and consistency of battery manufacturing. These steps constitute a closed-loop feedback process that helps to continuously optimize the production process and ensure the performance and safety of the final product.

[0111] In summary, this application reflects the true indentation depth by performing a depth scan on the embossing indentation and calculating the depth difference from the center point of the embossing to the edge. This method can provide more realistic and accurate measurement results, which helps to improve production quality and reduce defective product rates. By accurately controlling the embossing depth, the occurrence of lithium plating can be effectively avoided, thereby improving the overall performance and safety of the battery.

[0112] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for measuring embossing depth, characterized in that: The following steps are involved: a) preparing a two-dimensional microscope having a depth scanning function; b) placing the electrode with embossing to be tested on the workbench of the secondary microscope; c) using the microscope to perform a depth scan on the embossed indentation on the pole piece to obtain three-dimensional image information of the indentation; d) determining the center point position of the embossing in the three-dimensional image information; e) selecting at least one reference point from the center point to the edge of the indentation; f) measuring the depth difference between the reference point and the center point using the microscope; g) calculating the average depth of embossing according to the depth difference; h) analyzing the average depth data to assess whether the embossing is too deep; i) If the analysis results show that the embossing is too deep, the embossing process parameters are adjusted until the predetermined standards are met.

2. A method for measuring embossing depth according to claim 1, characterized in that: In step a), it also includes: a1) adjusting the illumination brightness of the microscope to ensure that the indentation outline is clearly visible; a2) setting the focal length of the microscope under lighting conditions to obtain the best focusing effect of the indentation; a3) calibrating the depth scanning range of the microscope according to the focal length setting; a4) activating the depth scanning function of the microscope, and starting to perform a depth scan of the indentation according to the calibration result in step a3).

3. A method for measuring embossing depth according to claim 1, characterized in that: In step b), it also includes: b1) Clean the electrode surface to remove impurities that may affect the depth measurement accuracy; b2) placing the cleaned electrode flat on the workbench of the microscope, and ensuring that the embossed surface faces upward; b3) adjusting the position of the pole piece in step b2) so that the embossing is located at the center of the observation field of the microscope; b4) Fixing the pole piece in step b2) to prevent it from moving during the depth scanning process.

4. A method for measuring embossing depth according to claim 1, characterized in that: In step c), it also includes: c1) adjusting the focus of the microscope to the embossed surface of the pole piece; c2) setting the scanning parameters of the microscope to adapt to the indentation characteristics on the pole piece; c3) performing the depth scan to obtain three-dimensional image information of the indentation on the pole piece; c4) recording the three-dimensional image information in step c3) for subsequent analysis and processing.

5. The method for measuring embossing depth according to claim 1, characterized in that: In step d), it also includes: d1) selecting an embossed area in the three-dimensional image information; d2) identifying the highest point in the embossing area in step d1) as the center point of the embossing; d3) marking the position coordinates of the center point in step d2) as a reference point for subsequent measurements; d4) recording the position coordinate information of the center point in step d3).

6. The method for measuring embossing depth according to claim 1, characterized in that: In step e), it also includes: e1) finding different directions around the center point in the three-dimensional image information; e2) selecting at least one direction from the different directions as the direction of the reference point; e3) finding the position of the edge of the indentation outward from the center point of step d) along the direction of step e2); e4) Marking the edge position in step e3) as a reference point and recording its coordinate information.

7. The method for measuring embossing depth according to claim 1, characterized in that: In step f), it also includes: f1) using the microscope to align the position of the reference point in step e); f2) measuring the vertical distance between the reference point in step f1) and the center point in step d); f3) determining the depth difference of the reference point relative to the center point according to the vertical distance in step f2); f4) recording the depth difference value in step f3).

8. The method for measuring embossing depth according to claim 1, characterized in that: In step g), it also includes: g1) collecting depth difference values ​​between each reference point and the center point in step f); g2) adding the depth difference values ​​in step g1) to obtain a total; g3) calculating the total number of depth difference values ​​in step g1); g4) The average depth of the embossing is obtained by dividing the sum in step g2) by the number in step g3).

9. The method for measuring embossing depth according to claim 1, characterized in that: In step h), it also includes: h1) comparing the average depth data in step g) with a preset standard depth threshold; h2) if the average depth in step h1) exceeds the standard depth threshold, it is judged that the embossing is too deep; h3) recording the judgment result in step h2); h4) taking corresponding process adjustment measures based on the recorded results in step h3).

10. The method for measuring embossing depth according to claim 1, characterized in that: In step i), it also includes: i 1) according to the analysis result in step h), if the embossing is too deep, adjusting the embossing process parameters; i2) re-performing steps b) to h) to verify the adjusted process parameters; i 3) comparing the verification result in step i2) with a predetermined standard; i4) If the verification result in step i3) does not meet the predetermined standard, repeat steps i1) to i3) until the predetermined standard is met.

Citation Information

Cited By

  • Method for measuring height and diameter of circular embossing based on three-dimensional vision

    CN120651117A