Preparation method of porous antireflection film, porous antireflection film and optical device
By preparing the metal organic composite layer on the substrate and forming a porous metal oxide layer to reinforce the model-retaining layer, the problems of complex and poor stability of the traditional porous urge membrane preparation process are solved, and efficient and controllable porous urge membrane preparation is achieved. , suitable for optical devices.
Patent Information
- Application Number
- CN202411232645.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-29
AI Technical Summary
The preparation process of traditional porous urge membranes is complex, with poor controllability of pore structures and insufficient stability, which limits its application in optical devices.
The metal organic composite layer is prepared on the substrate, and the porous metal oxide layer is formed through hydrolysis reaction, and the type-retaining layer is reinforced, so as to improve the controllability and stability of the pore structure through atomic layer deposition and other methods.
It realizes efficient preparation of porous urge membranes, improves the controllability and air stability of the pore structure, enhances friction resistance, and simplifies the process, which is suitable for large-area and regional selective generation.
Smart Images

Figure CN119045093A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thin films, and in particular to a method for preparing a porous anti-reflection film, the porous anti-reflection film and an optical device. Background Art
[0002] Optical anti-reflection film is an optical film with a very wide range of applications. Optical anti-reflection film is used to reduce the reflected light on the surface of optical devices and increase the light transmittance of optical devices. Traditional optical anti-reflection film uses the principle of interference destructive light to reduce reflected light and increase transmitted light. Traditional optical anti-reflection film usually includes dozens or even hundreds of layers of films with different refractive indices. These films increase the transmittance of light in a specific band by matching thickness and refractive index. The structure and preparation process of this optical anti-reflection film are relatively complex, and it can only achieve anti-reflection effect within a limited band, and its durability and stability are also poor.
[0003] A porous anti-reflection film is a porous anti-reflection film that uses the microporous structure of the material to reduce the reflection of light at the interface, thereby improving the transmittance. By rationally designing the microporous structure and adjusting the material parameters, the refractive index of light of a specific wavelength can be controlled, thereby achieving an effective anti-reflection effect. In traditional technologies, porous anti-reflection films are usually prepared by template method, sol-gel method or template method. Among them, the sol-gel method refers to the gelation of the precursor molecules in the sol in the presence of a gelling agent to form a solid material, and then heat treatment to form a pore structure. This method has a high process complexity and poor structural stability of the prepared material. The template method refers to the use of a template agent to form a pore structure, and then fill the material into the pore structure of the template, and finally remove the template agent to obtain a porous material. This method often requires the type of template agent to be changed when regulating the pore structure, and the process complexity is high and the controllability is poor. Therefore, traditional technologies often have problems such as high process complexity, insufficient controllability of the pore structure, and poor stability, which limits the further development and application of porous anti-reflection films. Summary of the invention
[0004] Based on this, it is necessary to provide a method for preparing a porous anti-reflection film in response to the problems in the above-mentioned background technology, which has low process complexity, can improve the controllability of the pore structure and take into account the stability of the pore structure.
[0005] According to some embodiments of the present disclosure, a method for preparing a porous anti-reflection film comprises the following steps:
[0006] Preparing at least one first precursor monolayer and at least one second precursor monolayer on a substrate, wherein the material of the first precursor monolayer and the material of the second precursor monolayer react to form a metal-organic composite layer capable of hydrolysis;
[0007] placing the metal-organic composite layer in an aqueous environment to perform a hydrolysis reaction, so that the metal-organic composite layer is transformed into a porous metal oxide layer; and
[0008] A conformal layer for reinforcing the porous metal oxide layer is prepared on the porous metal oxide layer.
[0009] In some embodiments of the present disclosure, the conformal layer is made of a material selected from oxides. The conformal layer is prepared by one or more methods selected from atomic layer deposition, molecular layer deposition, chemical vapor deposition, physical vapor deposition and liquid phase epitaxy.
[0010] In some embodiments of the present disclosure, the material of the conformal layer is selected from one or more of silicon oxide, aluminum oxide and titanium oxide.
[0011] In some embodiments of the present disclosure, the thickness of the conformal layer is ≤10 nm.
[0012] In some embodiments of the present disclosure, before preparing the conformal layer, a step of performing a conformal treatment on the porous metal oxide layer is also included.
[0013] In some embodiments of the present disclosure, the step of performing shaping treatment on the porous metal oxide layer includes: placing the porous metal oxide layer in a protective gas environment, and heating the porous metal oxide layer.
[0014] In some embodiments of the present disclosure, the process of heating the porous metal oxide layer satisfies at least one of the following characteristics:
[0015] (1) The heating temperature is 50℃~80℃;
[0016] (2) The heating time is 5min~10min.
[0017] In some embodiments of the present disclosure, the process of performing the hydrolysis reaction satisfies at least one of the following characteristics:
[0018] (1) The temperature of the hydrolysis reaction is 10℃~80℃;
[0019] (2) The hydrolysis reaction time is 5min~120min.
[0020] In some embodiments of the present disclosure, the thickness of the formed metal-organic composite layer is 5 nm to 60 nm.
[0021] In some embodiments of the present disclosure, the steps of preparing a first precursor monolayer and a second precursor monolayer on a substrate include:
[0022] placing the substrate in a deposition chamber;
[0023] Introducing the material of the first precursor monolayer into the deposition chamber and making it adhere to the substrate to form the first precursor monolayer;
[0024] Introducing the material of the second precursor monolayer into the deposition chamber and making it adhere to the substrate to form the second precursor monolayer;
[0025] The step of forming the first precursor monolayer and the step of forming the second precursor monolayer are taken as one deposition cycle, and the deposition cycles are repeated multiple times.
[0026] In some embodiments of the present disclosure, the metal-organic composite layer includes an aluminum-based organic-inorganic hybrid material; the material of the first precursor monolayer includes a metal-organic compound, and the material of the second precursor monolayer includes an alcohol organic substance and / or its derivatives.
[0027] In some embodiments of the present disclosure, the material of the first precursor monolayer includes trimethylaluminum, and the material of the second precursor monolayer includes one or more of ethylene glycol, glycerol and ethanolamine.
[0028] In some embodiments of the present disclosure, the process of preparing the first precursor monolayer and the second precursor monolayer on the substrate satisfies at least one of the following features:
[0029] (1) The number of deposition cycles is 15 to 100 times;
[0030] (2) The temperature of the deposition chamber is 50℃~200℃.
[0031] Furthermore, the present disclosure also provides a porous anti-reflection film, which includes a porous metal oxide layer and a conformal layer, wherein the conformal layer is attached to the pore structure of the porous metal oxide layer, and the porous anti-reflection film is prepared by the preparation method of the porous anti-reflection film described in any of the above embodiments.
[0032] In some embodiments of the present disclosure, the porous metal oxide layer satisfies at least one of the following characteristics:
[0033] (1) The thickness of the porous metal oxide layer is 40 nm to 100 nm;
[0034] (2) The pore size of the pores in the porous metal oxide layer is 35 nm to 105 nm;
[0035] (3) The average light transmittance of the porous metal oxide layer in the 450nm~675nm band is above 99%.
[0036] The present disclosure also provides an optical device, which includes a workpiece body and a porous anti-reflection film arranged on the workpiece body, wherein the porous anti-reflection film includes a porous anti-reflection film as described in any of the above embodiments. In the preparation method of the porous anti-reflection film of the present disclosure, a first precursor monolayer and a second precursor monolayer are first combined to form a metal organic composite layer. Then the metal organic composite layer is subjected to a hydrolysis reaction with water, so that the metal organic composite layer is converted into a porous metal oxide layer with a porous structure. Compared with the traditional preparation method of the porous anti-reflection film, the process complexity of the preparation method is significantly lower. The combination of the formation of the metal organic composite layer and the hydrolysis reaction thereof can effectively improve the controllability of the pore structure. On this basis, the further formed conformal layer can also improve the air stability and friction resistance of the porous metal oxide layer while basically not changing the pore structure, so that the prepared porous anti-reflection film also has a high stability.
[0037] In addition, thanks to the high consistency of the preparation method, the desired porous structure can be customized by selecting the materials of the first precursor monolayer and the second precursor monolayer, controlling the thickness of the metal-organic composite layer and the temperature and time of the hydrolysis reaction.
[0038] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, drawings of other embodiments can be obtained based on these drawings without creative work.
[0040] Figure 1 A schematic diagram of the steps of a method for preparing a porous anti-reflection film;
[0041] Figure 2 The left picture is a picture of the surface morphology of the sample before and after the setting treatment in Example 1 after being left standing in the air for a certain period of time, wherein the left picture is a picture of the surface morphology of the sample before the setting treatment after being left standing for 20 hours, and the right picture is a picture of the surface morphology of the sample after the setting treatment after being left standing for 100 hours;
[0042] Figure 3The surface morphology photos of the samples prepared in Example 1 and Comparative Example 1 after being wiped with steel wool, wherein the left picture is the surface morphology photo of the sample of Example 1 after being wiped, and the right picture is the surface morphology photo of the sample of Comparative Example 1 after being wiped;
[0043] Figure 4 The surface morphology of the sample of Example 1 observed by scanning electron microscope;
[0044] Figure 5 The surface morphology of the sample of Example 2 observed by scanning electron microscope;
[0045] Figure 6 The surface morphology of the sample of Example 3 observed by scanning electron microscope;
[0046] Figure 7 is a curve showing a change in transmittance versus incident light wavelength in Example 1, wherein the abscissa is wavelength in nm, and the ordinate is transmittance;
[0047] Figure 8 is a curve showing a change in transmittance versus incident light wavelength in Example 2, wherein the abscissa is wavelength in nm, and the ordinate is transmittance;
[0048] Fig. 9 3 is a curve showing the variation of transmittance with the wavelength of incident light in Example 3, wherein the abscissa is the wavelength in nm, and the ordinate is the transmittance. DETAILED DESCRIPTION
[0049] To facilitate understanding of the present invention, a more comprehensive description of the present invention is provided below. The preferred embodiments of the present invention are given herein. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the content of the present invention more thorough and comprehensive.
[0050] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this document pertains. The terms used herein in the specification of this document are only for describing specific embodiments and are not intended to limit this document.
[0051] It should be understood that when an element or layer is referred to as being "on, "adjacent to, "connected to, or "coupled to" another element or layer, it may be directly on, adjacent to, connected to, or coupled to the other element or layer, or there may be intervening elements or layers. In contrast, when an element is referred to as being "directly on, "directly adjacent to, "directly connected to, or "directly coupled to" another element or layer, there may be no intervening elements or layers. It should be understood that although the terms first, second, third, etc. may be used to describe various elements, components, regions, layers, and / or portions, these elements, components, regions, layers, and / or portions should not be limited by these terms. These terms are merely used to distinguish one element, component, region, layer, or portion from another element, component, region, layer, or portion.
[0052] Spatially relative terms such as "under," "beneath," "below," "under," "above," "above," and the like may be used herein for ease of description to describe the relationship of one element or feature to other elements or features. It should be understood that the spatially relative terms are intended to also include different orientations of the device in use and operation. For example, if the device in the accompanying drawings is flipped, then the elements or features described as "under other elements" or "under" or "under" will be oriented as "over" the other elements or features. Thus, the exemplary terms "under" and "under" may include both upper and lower orientations. The device may be otherwise oriented (e.g., rotated 90 degrees or other orientations) and the spatial descriptors used may be interpreted accordingly.
[0053] The purpose of the terms used herein is only to describe specific embodiments and is not intended to be a limitation of the present disclosure. When used herein, the singular forms "a", "an" and "the" are also intended to include plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "consisting of" and / or "comprising", when used in this specification, determine the presence of features, integers, steps, operations, elements and / or parts, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, parts and / or groups. When used herein, the term "and / or" includes any and all combinations of the relevant listed items.
[0054] The present disclosure provides a method for preparing a porous anti-reflection film, which comprises the following steps: preparing at least one first precursor monolayer and at least one second precursor monolayer on a substrate, wherein the material of the first precursor monolayer and the material of the second precursor monolayer react to form a metal organic composite layer capable of hydrolysis. The metal organic composite layer is placed in an aqueous environment for hydrolysis reaction, so that the metal organic composite layer is transformed into a porous metal oxide layer. Furthermore, a conformal layer for reinforcing the porous metal oxide layer is prepared on the porous metal oxide layer.
[0055] Among them, in the actual preparation process, the first precursor monolayer and the second precursor monolayer can be formed by attaching a monolayer molecule to the base material. It can be understood that the first precursor monolayer and the second precursor monolayer can be combined by chemical reaction to form a metal organic composite layer, and the material of the metal organic composite layer can be hydrolyzed and form the oxide of the metal. The hydrolysis reaction between the metal organic composite layer and water causes the material of the metal organic composite layer to gradually decompose, and causes the structural change of the metal organic composite layer, thereby generating a pore structure. The present disclosure found in the research process that the pore structure and pore size are closely related to the conditions of the hydrolysis reaction (such as time and temperature). By controlling the conditions of the hydrolysis reaction, the surface hydrolysis rate of the metal organic composite layer can be controlled, thereby achieving precise control of the pore structure and pore size in the porous metal oxide layer.
[0056] In the preparation method of the porous anti-reflection film disclosed in the present invention, the first precursor monolayer and the second precursor monolayer are first combined to form a metal organic composite layer. Since the first precursor monolayer and the second precursor monolayer are prepared and reacted as monolayers, the interference of random factors can be effectively avoided and it is easy to reproduce, so that the structure of the metal organic composite layer is highly controllable and reproducible. Then, the metal organic composite layer is hydrolyzed with water, so that the metal organic composite layer is converted into a porous metal oxide layer with a porous structure. The pore structure in the porous metal oxide layer is related to the structure and hydrolysis conditions of the metal organic composite layer. By controlling the hydrolysis conditions and the structure of the metal organic composite layer, the precise control of the pore structure and size can be achieved. Therefore, the combination of the formation of the metal organic composite layer and the hydrolysis reaction can effectively improve the controllability of the pore structure. On this basis, the further formed conformal layer can also improve the air stability and friction resistance of the porous metal oxide layer while substantially not changing the pore structure, so that the prepared porous anti-reflection film also has high stability.
[0057] Compared with the traditional preparation methods such as template method or sol-gel method, the preparation method of the porous anti-reflection film disclosed in the present invention is prepared by depositing molecular layers, which can realize the rapid, efficient and large-area preparation of the porous anti-reflection film. And the preparation process is more simplified and the preparation efficiency is higher. The preparation method of the porous anti-reflection film disclosed in the present invention can be prepared on a variety of different substrates, and combined with the selective deposition technology, the regional selective generation of the porous anti-reflection film can also be achieved to meet different application requirements. Furthermore, after experimental verification, the porous anti-reflection film prepared by the preparation method of the porous anti-reflection film disclosed in the present invention also has an excellent anti-reflection effect.
[0058] Figure 1 Schematic diagram of the steps of a method for preparing a porous antireflection film disclosed in the present invention. Figure 1As shown, the method for preparing the porous anti-reflection film includes steps S1 to S3, which are specifically as follows.
[0059] Step S1, preparing at least one first precursor monolayer and at least one second precursor monolayer on a substrate.
[0060] As some examples of this embodiment, the substrate may be a workpiece on which a porous antireflection film is to be prepared. The workpiece may be, but is not limited to, an optical lens. The material of the optical lens may be organic glass or inorganic glass. As an example, the organic glass is resin glass, and the inorganic glass is K9 glass.
[0061] In this embodiment, the material of the first precursor monolayer and the material of the second precursor monolayer react to form a metal-organic composite layer that can be hydrolyzed. The metal-organic composite layer contains a metal-organic composite material, which refers to a material formed by the combination of metal atoms and carbon chains of organic matter. During hydrolysis, the metal atoms can combine with hydroxyl groups in water to form metal-hydroxyl compounds, and finally form metal oxides.
[0062] As some examples of this embodiment, the metal-organic composite layer includes an aluminum-based organic-inorganic hybrid material.
[0063] It is understood that the materials of the first precursor monolayer and the second precursor monolayer can be selected according to the desired metal organic composite layer. As some examples of this embodiment, the first precursor monolayer includes metal organic compounds, and the second precursor monolayer includes alcohol organics and / or their derivatives.
[0064] As some examples of this embodiment, in the first precursor monolayer, the metal organic compound can be an alkyl metal compound. In this example, the metal atom in the alkyl metal compound can be selected from one or more of aluminum, gallium, indium, tin, lead, zinc, titanium and cobalt. In this example, according to the coordination number of the metal atom in the alkyl metal compound, the alkyl group can have one or more. The alkyl group can be selected from an alkyl group with a carbon number of 1 to 20, for example, the alkyl group can be a methyl group, an ethyl group, a propyl group, a butyl group, etc.
[0065] Further, the metal organic compound in the first precursor monomolecular layer is trimethylaluminum. It is understood that in other examples, the metal organic compound may also be but not limited to triethylaluminum, tetramethyltin and dimethylzinc.
[0066] Furthermore, the alcohol organic substance in the second precursor monomolecular layer can be selected from one or more of ethylene glycol, glycerol and ethanolamine.
[0067] In other examples, the alcohol organic compound may also be selected from one or more diols such as propylene glycol, butanediol and pentanediol. The derivative of the alcohol organic compound refers to an alcohol organic compound in which at least one hydrogen atom is replaced.
[0068] Taking trimethylaluminum and diol as an example, trimethylaluminum and diol can react to form an alkoxy aluminum compound, and the alkoxy aluminum compound is used as the material of the metal organic composite layer.
[0069] As some examples of this embodiment, the first precursor monolayer and the second precursor monolayer both have multiple layers. It can be understood that by providing multiple layers of the first precursor monolayer and multiple layers of the second precursor monolayer, a thicker metal organic composite layer can be formed. In addition, by controlling the number of layers of the first precursor monolayer and the second precursor monolayer, the thickness of the formed metal organic composite layer can be controlled. This is also conducive to achieving precise control of the overall structure of the final porous metal oxide layer.
[0070] As some examples of this embodiment, the steps of preparing a first precursor monolayer and a second precursor monolayer on a substrate include: placing the substrate in a deposition chamber. Passing the material of the first precursor monolayer into the deposition chamber and attaching it to the substrate to form the first precursor monolayer. Passing the material of the second precursor monolayer into the deposition chamber and attaching it to the substrate to form the second precursor monolayer. The steps of forming the first precursor monolayer and the steps of forming the second precursor monolayer are regarded as a deposition cycle, and the deposition cycles are repeated multiple times.
[0071] For example, a first precursor monolayer is first formed on a substrate, and the first precursor monolayer is attached to the substrate. Then, a second precursor monolayer is formed, and the second precursor monolayer is attached to the first precursor monolayer prepared earlier and reacts with it. Then, the first precursor monolayer and the second precursor monolayer are alternately deposited until a preset number of layers is reached. The first precursor monolayer deposited later is attached to the second precursor monolayer deposited earlier, and the second precursor monolayer deposited later is also attached to the first precursor monolayer deposited earlier. Multiple first precursor monolayers and multiple second precursor monolayers are combined to form a metal organic composite layer.
[0072] As some examples of this embodiment, after each formation of the first precursor monolayer and the second precursor monolayer, a step of purging the deposition chamber may be included. The step of purging the deposition chamber includes: introducing a protective gas into the deposition chamber to remove unreacted materials and byproducts generated by the reaction, ensuring the purity of the surface, and ensuring the continuous deposition.
[0073] It can be understood that, in this embodiment, the process of preparing the first precursor monolayer and the second precursor monolayer on the substrate can be performed using a molecular layer deposition (Molecular Layer Deposition) device.
[0074] As some examples of this embodiment, the thickness of the formed metal-organic composite layer is 5 nm to 60 nm.
[0075] In this example, the thickness of the metal organic composite layer is 5nm, 10nm, 15nm, 20nm, 25nm, 30nm, 35nm, 40nm, 45nm, 50nm, 55nm, 60nm. Alternatively, the thickness of the metal organic composite layer can also be between any two of the above thicknesses. The metal organic composite layer of the above thickness is conducive to forming a porous metal oxide layer with a relatively stable pore structure and good light transmission performance during the subsequent hydrolysis process.
[0076] It is understood that the thickness of the metal-organic composite layer can be controlled by controlling the number of deposition cycles.
[0077] As some examples of this embodiment, the number of deposition cycles may be 15 to 100 times. That is, 15 to 100 layers of the first precursor monolayer and 15 to 100 layers of the second precursor monolayer are alternately deposited. For example, the number of deposition cycles may be 15, 20, 25, 30, 40, 50, 60, 70, 80, 90, 100 times, or the number of deposition cycles may be between any two of the above numbers.
[0078] As some examples of this embodiment, during the process of forming the first precursor monolayer and the second precursor monolayer, the temperature of the deposition chamber is 50° C. to 200° C. Controlling the temperature of the deposition chamber within this range helps to make the first precursor monolayer adhere more fully and evenly, and makes the process of combining the first precursor monolayer with the second precursor monolayer to form a metal-organic composite layer more controllable, thereby improving the controllability of the pore structure in the subsequently formed porous metal oxide layer.
[0079] In the preparation method, the first precursor monolayer and the second precursor monolayer can be deposited at a relatively low temperature, and thus are particularly suitable for preparation on certain substrates with poor high temperature resistance. For substrates with poor high temperature resistance, during the formation of the first precursor monolayer and the second precursor monolayer, the temperature of the deposition chamber can be 50°C to 100°C. For example, the temperature of the deposition chamber can be 50°C, 60°C, 70°C, 80°C, 90°C, or 100°C. Alternatively, the temperature of the deposition chamber can also be between any two of the above temperatures.
[0080] Step S2, placing the metal-organic composite layer in an aqueous environment to perform a hydrolysis reaction, so that the metal-organic composite layer is transformed into a porous metal oxide layer.
[0081] In this embodiment, the material of the porous metal oxide layer includes metal oxide, and the metal element in the metal oxide is the metal element in the metal-organic composite layer.
[0082] As some examples of this embodiment, the metal-organic composite layer may be placed in water to perform a hydrolysis reaction. Alternatively, in other examples, the metal-organic composite layer may be placed in a humid gas environment containing water vapor to perform a hydrolysis reaction.
[0083] Taking the hydrolysis reaction of alkoxy aluminum compounds as an example, alkoxy aluminum compounds (Al-O-CH2-CH2-O-Al) react with water to form hydroxy aluminum compounds (Al-OH), and the chemical reaction formula is as follows: Al-O-CH2-CH2-O-Al+H2O→Al-OH+HO-CH2-CH2-O-Al. The hydroxy aluminum compounds are further dehydrated to form aluminum oxide. In addition, the hydroxyl groups can also produce alcoholate ions RO during hydrolysis. - (R represents the group connected to the hydroxyl group), the chemical reaction formula is as follows: ROH+H2O→RO - +H3O + , the alcoholate ion can further react with water in the presence of carbon dioxide to produce carboxylic acid (RCOOH), the chemical reaction formula is as follows: RO - +CO+H2O→RCOOH+OH - Therefore, after the hydrolysis reaction, the alkoxide aluminum polymer can gradually transform into a porous aluminum oxide material containing hydroxyl and carboxyl functional groups on the surface.
[0084] As some examples of this embodiment, during the hydrolysis reaction, the temperature of the hydrolysis reaction can be controlled to be 10°C to 80°C. Controlling the temperature of the hydrolysis reaction can obtain a more optimized hydrolysis reaction rate, which is conducive to more accurate control of the obtained pore structure. When the temperature of the hydrolysis reaction is low, the hydrolysis reaction rate is too slow, which is not conducive to the formation of a porous structure. When the temperature of the hydrolysis reaction is high, the hydrolysis reaction rate is too fast, which is not conducive to more accurate control of the porous structure.
[0085] In this example, the temperature of the hydrolysis reaction can be controlled to 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 50°C, 60°C, 70°C, or 80°C, or the temperature of the hydrolysis reaction can be controlled between any two of the above temperatures.
[0086] As some examples of this embodiment, the time of the hydrolysis reaction can be controlled to be 5 minutes to 120 minutes. Controlling the time of the hydrolysis reaction is conducive to controlling the progress of the hydrolysis reaction, and can achieve regulation of the pore size, shape and arrangement, so as to prepare a porous metal oxide layer with a controllable pore structure. And the time of the hydrolysis reaction is also conducive to obtaining a porous metal oxide layer with significantly higher transmittance.
[0087] In this example, the time of the hydrolysis reaction can be controlled to be 5 min, 10 min, 15 min, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min. Alternatively, the time of the hydrolysis reaction can be controlled to be between any two of the above times.
[0088] It is understood that when the temperature of the hydrolysis reaction is higher, the hydrolysis reaction rate is faster, and the time of the hydrolysis reaction can be controlled to be shorter, that is, the required pore structure can be formed. When the temperature of the hydrolysis reaction is lower, the hydrolysis reaction rate is slower, and the time of the hydrolysis reaction can be controlled to be longer at this moment, to form the required pore structure. In addition, the time of the hydrolysis reaction can also be controlled according to the thickness of the metal organic composite layer. For example, for a thicker metal organic composite layer, a longer hydrolysis reaction time can be adopted to ensure that the metal organic composite layer can be more fully hydrolyzed and converted into a porous metal oxide layer.
[0089] As some examples of this embodiment, after the hydrolysis reaction, the method further includes a step of drying the formed porous metal oxide layer, wherein the drying process is used to remove the residual water in the porous metal oxide layer.
[0090] In this example, the drying process is performed by purging the porous metal oxide layer with a protective gas.
[0091] In this embodiment, the pore structure of the porous metal oxide layer produced by the hydrolysis reaction still has the problem of poor stability, which causes the pore structure of the layer to be easily destroyed and easily fall off from the surface of the substrate. As some examples of this embodiment, after forming the porous metal oxide layer, the step of shaping the porous metal oxide layer may also be included.
[0092] In this example, the step of shaping the porous metal oxide layer includes placing the porous metal oxide layer in a protective gas environment and heating the porous metal oxide layer. By heating the porous metal oxide layer, the pore structure therein can be shaped and the bonding strength between the porous metal oxide layer and the substrate can be enhanced.
[0093] In this example, when the porous metal oxide layer is heated, the heating temperature is 50° C. to 80° C. For example, the heating temperature may be 50° C., 55° C., 60° C., 65° C., 70° C., 75° C., or 80° C., or the heating temperature may be in a range between any two of the above temperatures.
[0094] As some examples of this embodiment, when the porous metal oxide layer is heated, the heating time is 5 minutes to 10 minutes. For example, the heating time can be 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, or the heating time can also be in the range between any two of the above times.
[0095] Step S3, preparing a conformal layer on the porous metal oxide layer for reinforcing the porous metal oxide layer.
[0096] In this embodiment, the conformal layer covers the surface of the porous metal oxide layer. It can be understood that the surface of the porous metal oxide layer is porous, and the conformal layer can be attached to the pore walls therein. The conformal layer can reinforce the pore structure of the porous metal oxide layer, so that the porous metal oxide layer can maintain the pore structure when facing external forces such as friction. And the conformal layer also enables the porous metal oxide layer to be stably attached to the substrate.
[0097] As some examples of this embodiment, the material of the conformal layer is selected from oxides. The oxides have similar material structures to the porous metal oxide layer, which enables the conformal layer to be more closely combined with the porous metal oxide layer.
[0098] In this example, the material of the conformal layer may be selected from one or more of titanium dioxide, aluminum oxide, and silicon dioxide.
[0099] In this example, the material of the conformal layer is the same as that of the porous metal oxide layer.
[0100] As some examples of this embodiment, the thickness of the conformal layer is ≤10nm. Using a conformal layer with a thickness of less than 10nm can avoid the conformal layer filling up the pore structure as much as possible and maintain the original pore structure in the porous metal oxide layer. Optionally, the thickness of the conformal layer can be 1nm~3nm. This is conducive to obtaining better conformal performance while substantially not changing the pore structure.
[0101] In this example, the thickness of the conformal layer may be 1 nm, 1.5 nm, 2 nm, 2.5 nm, or 3 nm, or the thickness of the conformal layer may be between any two of the above thicknesses.
[0102] As some examples of this embodiment, the method of preparing the conformal layer on the porous metal oxide layer is selected from one or more of chemical vapor deposition (CVD), physical vapor deposition (PVD), atomic layer deposition (ALD), molecular layer deposition and liquid phase epitaxy. Preferably, the atomic layer deposition method can be used to prepare a thinner and more uniform conformal layer, which can provide better conformal ability while minimizing the impact on light transmission performance.
[0103] It can be understood that through steps S1 to S3, a porous anti-reflection film can be prepared.
[0104] Furthermore, the present disclosure also provides a porous anti-reflection membrane, which can be prepared by the preparation method in the above embodiment.
[0105] As some examples of this embodiment, a porous antireflection film includes a porous metal oxide layer and a conformal layer attached to the pore walls of the porous metal oxide layer, wherein the porous metal oxide layer can be prepared by the preparation method in the above embodiment.
[0106] As some examples of this embodiment, the average transmittance of the porous anti-reflection film in the 450nm~675nm band is above 99%.
[0107] As some examples of this embodiment, the thickness of the porous metal oxide layer is 40 nm to 100 nm.
[0108] As some examples of this embodiment, the pore diameter of the holes in the porous metal oxide layer is 35 nm to 105 nm.
[0109] Furthermore, the present disclosure also provides an optical device, which includes a workpiece body and a porous anti-reflection film disposed on the workpiece body. The porous anti-reflection film is the porous anti-reflection film in the above embodiment.
[0110] As some examples of this embodiment, the optical device may be an imaging device, such as a display, the workpiece body of the display includes a panel glass, and the porous anti-reflection film may be disposed on the panel glass of the display.
[0111] As some examples of this embodiment, the optical device may be a projection device, such as a projector, the workpiece body of the projector includes a lens, and the porous anti-reflection film may be disposed on the lens of the projector.
[0112] As some examples of this embodiment, the optical device may further include an imaging device, such as a camera, the workpiece body of the camera includes a lens, and the porous anti-reflection film may be disposed on the lens.
[0113] The present disclosure also provides the following examples to further illustrate some implementations of the above preparation method. Accordingly, the present disclosure also provides the following comparative examples to illustrate the advantages of the preparation method.
[0114] Example 1
[0115] K9 glass is used as a substrate, and the substrate is placed in a deposition chamber of a molecular layer deposition device.
[0116] The temperature in the deposition chamber is controlled at 120°C, trimethylaluminum is introduced into the deposition chamber to make it adhere to the substrate to form a first precursor monolayer, and then argon gas is introduced into the deposition chamber to purge the deposition chamber to remove unattached trimethylaluminum and other byproducts. Ethylene glycol is then introduced into the deposition chamber to make it adhere to the first precursor monolayer, and then argon gas is introduced into the deposition chamber to purge the deposition chamber to remove unattached ethylene glycol and other byproducts. The steps of introducing trimethylaluminum and ethylene glycol are repeated 50 times to form an alkoxide aluminum polymer as a metal organic composite layer.
[0117] The substrate was immersed in pure water for hydrolysis reaction, the water temperature was controlled at 50°C, the hydrolysis time was 45 minutes, and a porous metal oxide layer was formed. After hydrolysis, it was taken out and purged with a nitrogen gun for 2 minutes until there was no residual water stain on the surface.
[0118] The substrate was transferred to an oven at 75° C. and heated for 10 min to fix the pore structure.
[0119] The substrate was transferred to a deposition chamber of an atomic layer deposition device, and an aluminum oxide material with a thickness of 2 nm was deposited as a conformal layer.
[0120] Example 2
[0121] Example 2 is substantially the same as Example 1, except that: when preparing the metal organic composite layer, the step of introducing trimethylaluminum and ethylene glycol is repeated 75 times; when performing the hydrolysis reaction, the water temperature is controlled at 30° C. and the hydrolysis time is 60 min.
[0122] Example 3
[0123] Example 3 is basically the same as Example 1, except that: when preparing the metal organic composite layer, the step of introducing trimethylaluminum and ethylene glycol is repeated 40 times; when performing the hydrolysis reaction, the water temperature is controlled at 10° C. and the hydrolysis time is 100 min.
[0124] Example 4
[0125] Example 4 is basically the same as Example 1, except that: polymethyl methacrylate is used as the substrate; when preparing the metal organic composite layer, the step of introducing trimethylaluminum and ethylene glycol is repeated 80 times; when performing the hydrolysis reaction, the water temperature is controlled at 30°C and the hydrolysis time is 60 minutes.
[0126] Example 5
[0127] Example 5 is basically the same as Example 1, with the only difference being that: when preparing the metal-organic composite layer, propylene glycol is used instead of ethylene glycol, and the steps of introducing trimethylaluminum and propylene glycol are repeated 100 times; when conducting the hydrolysis reaction, the water temperature is controlled at 50°C and the hydrolysis time is 30 minutes; when preparing the conformal layer, a titanium dioxide material with a thickness of 2 nm is deposited.
[0128] Example 6
[0129] Example 6 is basically the same as Example 1, with the only difference being that polycarbonate is used as the substrate; when preparing the metal organic composite layer, ethanolamine is used instead of ethylene glycol, and the steps of introducing trimethylaluminum and ethanolamine are repeated 90 times; when performing the hydrolysis reaction, the water temperature is controlled at 80°C and the hydrolysis time is 5 minutes; when preparing the conformal layer, a silicon dioxide material with a thickness of 2 nm is deposited.
[0130] Example 7
[0131] Example 7 is basically the same as Example 1, with the only difference being that when preparing the conformal layer, the substrate is transferred to a deposition chamber of a chemical vapor deposition device, and a 2 nm thick aluminum oxide material is deposited by chemical vapor deposition.
[0132] Example 8
[0133] Example 8 is basically the same as Example 1, with the only difference being that when preparing the conformal layer, the substrate is transferred to a deposition chamber of a magnetron sputtering device, and a 2 nm thick aluminum oxide material is deposited by magnetron sputtering.
[0134] Example 9
[0135] Example 9 is substantially the same as Example 1, with the only difference being that when preparing the conformal layer, an aluminum oxide material with a thickness of 5 nm is deposited.
[0136] Example 10
[0137] Example 10 is substantially the same as Example 1, except that when preparing the conformal layer, an aluminum oxide material with a thickness of 0.5 nm is deposited.
[0138] Embodiment 11
[0139] Example 11 is substantially the same as Example 1, except that after hydrolysis and before the shape-retaining layer is prepared, no heating step is performed to fix the pore structure.
[0140] Example 12
[0141] Example 12 is substantially the same as Example 1, except that the hydrolysis temperature is 100°C.
[0142] Embodiment 13
[0143] Example 13 is substantially the same as Example 1, except that the hydrolysis time is 200 min.
[0144] Comparative Example 1
[0145] Comparative Example 1 is substantially the same as Example 1, except that after heating to fix the pore structure, the step of preparing the shape-retaining layer is not performed.
[0146] Comparative Example 2
[0147] Comparative Example 2 is basically the same as Example 1, except that after the metal organic composite layer is prepared, the substrate is directly transferred to a muffle furnace and heated to 500° C. in an air atmosphere for calcination, and then an aluminum oxide material with a thickness of 2 nm is deposited on the surface of the calcined material.
[0148] Test 1: Take two samples of Example 1 before and after the shaping treatment, respectively, and observe the surface morphology of the samples under a microscope after standing in the air for a certain period of time. The results can be seen in Figure 2 . Figure 2 The left picture in the figure is the surface morphology of the sample before the shaping treatment and after standing for 20 hours. Figure 2 The right picture in the figure is a photograph of the surface morphology of the sample after the shaping treatment after standing for 100 hours.
[0149] Reference Figure 2 As shown in the figure, before the shaping treatment, the film layer on the substrate surface has local bubbling, cracking and shedding after 20 hours, but after the shaping treatment, even after 100 hours, there is still no obvious abnormality in the film layer on the substrate surface. This shows that the heating and baking method can effectively stabilize the pore structure of the porous metal oxide layer.
[0150] Test 2: Take the samples prepared in Example 1 and Comparative Example 1, wipe them with steel wool, and observe the changes in the surface morphology of the samples under a microscope. The results can be seen in Figure 3 . Figure 3 The left picture in the figure is a photo of the surface morphology of the sample of Example 1 after wiping. Figure 3 The right picture in the figure is a photograph of the surface morphology of the sample of Comparative Example 1 after wiping.
[0151] Reference Figure 3 As shown, the surface film layer of Comparative Example 1 did not prepare a conformal layer, and bubbling, cracking, and shedding occurred after wiping. Compared with Comparative Example 1 in which a conformal layer was not further prepared, Example 1 further prepared a conformal layer on the basis of the porous metal oxide layer, and even after wiping with steel wool, the surface film layer of Example 1 still did not have the problem of bubbling and shedding. This shows that the design of the conformal layer structure can effectively ensure the structural stability of the porous metal oxide layer.
[0152] Experiment 3: The surface morphology of the samples of Example 1 to Example 3 was observed using a scanning electron microscope. The results can be seen in Figure 4~Figure 6 .in, Figure 4 is the surface morphology of the sample of Example 1, Figure 5 is the surface morphology of the sample of Example 2, Figure 6 This is the surface morphology of the sample of Example 3.
[0153] Reference Figure 4~Figure 6 As shown, Examples 1 to 3 respectively use different deposition cycles and different hydrolysis conditions, and all of them can prepare a porous metal oxide layer with a specific pore structure. Figure 4 In the porous structure, the pore size distribution is between 35nm and 105nm. Figure 5 In the porous structure, the pore size distribution is between 62nm and 90nm. Figure 6 In the embodiment 1, the pore size distribution of the porous structure is between 75nm and 95nm. This shows that the pore structure is related to the thickness of the metal organic composite layer and the hydrolysis conditions, and also shows that the pore structure can be correspondingly controlled by controlling the thickness of the metal organic composite layer and the hydrolysis conditions. Furthermore, the hydrolysis temperature of Example 1 is 50°C. Since the hydrolysis temperature is high and the hydrolysis rate is fast, it can be hydrolyzed more fully after 45 minutes of hydrolysis. However, the correspondingly formed pore size is more uneven, so the pore size distribution range is larger. The hydrolysis temperature of Example 2 is 30°C, and it is hydrolyzed more fully after 60 minutes of hydrolysis. The uniformity of its pore size is improved, and the pore size distribution range is reduced compared with Example 1. The hydrolysis temperature of Example 3 is 10°C, the hydrolysis rate is slower, and it takes 100 minutes of hydrolysis to be hydrolyzed more fully. The uniformity of its pore size is higher than that of Example 2, and the pore size distribution range is further reduced compared with Example 2.
[0154] Experiment 4: The average transmittance of the porous antireflection films prepared in each embodiment and comparative example between 450nm and 675nm was tested. The surface morphology of each embodiment and comparative example was observed after standing in air for 20h, and then the surface was wiped with steel wool and the surface morphology was observed again. The results can be seen in Table 1. The curves of the transmittance of Examples 1 to 3 as a function of the wavelength of the incident light are shown in Table 1. Figure 7~Figure 9 .
[0155] Table 1
[0156]
[0157] In the column of surface morphology after standing in Table 1, "√" indicates that the film is flat and has no cracking abnormalities, and "○" indicates that there are a few cracks on the surface of the film. In the column of surface morphology after wiping in Table 1, "√" indicates that the film has no bubbling or shedding problems, "○" indicates that the film has a little bubbling or shedding, and "×" indicates that the film has a large area of bubbling or shedding.
[0158] Reference Figure 7~Figure 9 As shown in Table 1, the average transmittance of the porous antireflection films prepared in Examples 1 to 3 in the 450nm~675nm band can be maintained above 99%. Referring to Table 1, the average transmittance of the porous antireflection films prepared in Examples 1 to 6 can reach above 99%, indicating that the preparation method disclosed in the present invention can prepare a porous antireflection film with a transmittance of above 99% by hydrolyzing the metal organic composite layer and then preparing the conformal layer.
[0159] Further, in Table 1, compared with Example 1, Comparative Example 1 did not prepare a conformal layer. Although Example 1 and Comparative Example 1 had similar average transmittances, there was a problem of large-area bubbling and shedding on the surface of Comparative Example 1, resulting in the film of Comparative Example 1 being unsuitable for practical use. This also shows that the use of atomic layer deposition to form a thin conformal layer does not have a significant negative impact on the transmittance of the porous metal oxide layer. Although Comparative Example 2 can form a porous metal oxide layer by direct calcination, the transmittance of the prepared film is significantly low. This also shows that the preparation method disclosed in the present invention can prepare a porous anti-reflection film with significantly higher transmittance.
[0160] In addition, refer to Example 1, Example 12 and Example 13. Compared with Example 1, Example 12 uses a higher hydrolysis temperature, and Example 13 uses a longer hydrolysis time, both of which reduce the transmittance of the porous anti-reflection film. This is mainly because the degree of hydrolysis is too deep, which has a certain negative impact on the transmittance of the porous structure.
[0161] Refer to Example 1 and Example 11. Compared with Example 1, Example 11 did not perform baking before preparing the conformal layer, resulting in a few cracks on the surface after placement, which not only had a certain negative impact on the structural stability of the porous anti-reflection film, but also caused the transmittance of the porous anti-reflection film to decrease.
[0162] Refer to Example 1 and Example 7 and Example 8. The transmittance of Example 7 and Example 8 is significantly lower than that of Example 1. This is mainly because Example 7 uses chemical vapor deposition to prepare the conformal layer, and Example 8 uses physical vapor deposition to prepare the conformal layer. The uniformity of the conformal layers prepared by the two is poor, which affects the original transmittance of the porous structure.
[0163] Refer to Example 1, Example 9 and Example 10. The conformal layer of Example 9 is slightly thicker, which has a certain negative impact on the light transmission performance of the pore structure, resulting in a decrease in the light transmittance of the porous anti-reflection film. The conformal layer of Example 10 is slightly thinner. Although the light transmittance of its porous anti-reflection film is basically the same as that of Example 1, the film is prone to a little bubbling and falling off after wiping, and the structural stability is slightly poor.
[0164] Please note that the above embodiments are for illustrative purposes only and are not meant to be limiting of this document.
[0165] It should be understood that, unless otherwise specified herein, there is no strict order restriction for the execution of the steps, and the steps may be executed in other orders. Moreover, at least a portion of the steps in the preparation process may include multiple sub-steps or multiple stages, and these sub-steps or stages are not necessarily executed at the same time, but may be executed at different times, and the execution order of these sub-steps or stages is not necessarily sequential, but may be executed in turn or alternately with other steps or at least a portion of the sub-steps or stages of other steps.
[0166] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.
[0167] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
Claims
1. A method for preparing a porous antireflection film, characterized in that: The steps include: Preparing at least one first precursor monolayer and at least one second precursor monolayer on a substrate, wherein the material of the first precursor monolayer and the material of the second precursor monolayer react to form a metal-organic composite layer capable of hydrolysis; placing the metal-organic composite layer in an aqueous environment to undergo a hydrolysis reaction, so that the metal-organic composite layer is converted into a porous metal oxide layer; and A conformal layer for reinforcing the porous metal oxide layer is prepared on the porous metal oxide layer.
2. The method for preparing a porous antireflection film according to claim 1, wherein: The material of the conformal layer is selected from oxides; the conformal layer is prepared by one or more methods selected from atomic layer deposition, molecular layer deposition, chemical vapor deposition, physical vapor deposition and liquid phase epitaxy.
3. The method for preparing a porous antireflection film according to claim 1, wherein: The material of the conformal layer is selected from one or more of silicon oxide, aluminum oxide and titanium oxide.
4. The method for preparing a porous antireflection film according to claim 1, wherein: The thickness of the conformal layer is ≤10 nm.
5. The method for preparing a porous antireflection film according to any one of claims 1 to 4, wherein: Before preparing the shape-preserving layer, the method further includes a step of performing a shape-fixing treatment on the porous metal oxide layer.
6. The method for preparing a porous antireflection film according to claim 5, wherein: The step of performing shaping treatment on the porous metal oxide layer comprises: placing the porous metal oxide layer in a protective gas environment, and heating the porous metal oxide layer.
7. The method for preparing a porous antireflection film according to claim 6, wherein: The process of heating the porous metal oxide layer satisfies at least one of the following characteristics: (1) The heating temperature is 50℃~80℃; (2) The heating time is 5 minutes to 10 minutes.
8. The method for preparing a porous antireflection film according to any one of claims 1 to 4 and 6 to 7, wherein: The process of performing the hydrolysis reaction satisfies at least one of the following characteristics: (1) The temperature of the hydrolysis reaction is 10℃~80℃; (2) The hydrolysis reaction time is 5min~120min.
9. The method for preparing a porous antireflection film according to any one of claims 1 to 4 and 6 to 7, wherein: The thickness of the formed metal-organic composite layer is 5nm-60nm.
10. The method for preparing a porous antireflection film according to claim 9, wherein: The steps of preparing a first precursor monolayer and a second precursor monolayer on a substrate include: placing the substrate in a deposition chamber; introducing the material of the first precursor monolayer into the deposition chamber and causing it to adhere to the substrate to form the first precursor monolayer; introducing the material of the second precursor monolayer into the deposition chamber and allowing the material to adhere to the substrate to form the second precursor monolayer; The step of forming the first precursor monolayer and the step of forming the second precursor monomolecule are taken as one deposition cycle, and the deposition cycles are repeated multiple times.
11. The method for preparing a porous antireflection film according to claim 10, wherein: The metal-organic composite layer includes an aluminum-based organic-inorganic hybrid material; the material of the first precursor monomolecular layer includes a metal-organic compound, and the material of the second precursor monomolecular layer includes an alcohol organic compound and / or its derivatives.
12. The method for preparing a porous antireflection film according to claim 11, wherein: The material of the first precursor monolayer includes trimethylaluminum, and the material of the second precursor monolayer includes one or more of ethylene glycol, glycerol, and ethanolamine.
13. The method for preparing a porous antireflection film according to any one of claims 10 to 12, characterized in that: The process of preparing the first precursor monolayer and the second precursor monolayer on the substrate satisfies at least one of the following characteristics: (1) The number of deposition cycles is 15 to 100; (2) The temperature of the deposition chamber is 50°C~200°C.
14. A porous antireflection film, characterized in that: The porous antireflection film comprises a porous metal oxide layer and a conformal layer, wherein the conformal layer is attached to the pore structure of the porous metal oxide layer, and the porous antireflection film is prepared by the preparation method of the porous antireflection film according to any one of claims 1 to 13.
15. The porous antireflection film according to claim 14, characterized in that: The porous metal oxide layer satisfies at least one of the following characteristics: (1) The thickness of the porous metal oxide layer is 40 nm to 100 nm; (2) The pores in the porous metal oxide layer have a pore diameter of 35 nm to 105 nm; (3) The average light transmittance of the porous metal oxide layer in the 450nm~675nm band is above 99%.
16. An optical device, characterized in that: The invention comprises a workpiece body and a porous antireflection film arranged on the workpiece body, wherein the porous antireflection film comprises the porous antireflection film according to any one of claims 14 to 15.
Citation Information
Cited By
Optical device, and preparation method therefor and use thereof
WO2026051884A1