LED chip, preparation method thereof and light-emitting equipment
By designing the N-type current expansion layer in the LED chip, using heavy doping and spaced doping technology, the problems of non-conductivity of the sapphire substrate and doping inhomogeneity of the N-type GaN layer are solved, and the photoelectricity of the LED chip is improved Performance and stability enhance current expansion and antistatic capabilities.
Patent Information
- Application Number
- CN202411248770.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-29
AI Technical Summary
The non-conductivity of the sapphire substrate makes it difficult for the production of the electrode of the LED chip, causing the current to flow laterally, affecting the emission efficiency of light, and the doping unevenness of the N-type GaN layer leads to a high resistance effect, reducing the stability of the LED chip.
An LED chip is designed, including an N-type current expansion layer on one side of the substrate, and by stacking a first N-type GaN layer, an N-type AlGaN layer and a superlattice structure arranged in the first direction, heavy doping and Spaced doping reduces contact barriers, improves lateral flow and longitudinal expansion capabilities, reduces dislocations, and forms an efficient current expansion layer.
It improves the photoelectric performance and stability of the LED chip, reduces the generation of thermal effects, enhances the current expansion ability, improves the output optical power and anti-static ability, and suppresses reverse leakage.
Smart Images

Figure CN119050224A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor technology, and in particular to an LED chip and a preparation method thereof, and a light-emitting device. Background Art
[0002] Sapphire substrates have many advantages over other substrates, but since sapphire substrates are not conductive, it is very difficult to make electrodes for LED chips. The more mature method now is to make a vertical electrode structure on the same side of the sapphire. This method requires etching on the surface of the material. When current is injected, the current does not flow vertically, but needs to flow horizontally. Since the electrode structure will affect the effective emission of light, the size of the electrode cannot be very large, which determines that the electrode structure cannot have a strong current expansion capability.
[0003] For conventional N-type GaN layers, if the doping is uneven, a high resistance effect will be formed locally. When a large current flows through it, a thermal effect will be generated, which will in turn destroy the PN junction structure and reduce the stability of the LED chip. Summary of the invention
[0004] In view of the above problems, the present application provides an LED chip and a preparation method thereof, and a light-emitting device, which improve the photoelectric performance and stability of the LED chip. The specific solution is as follows:
[0005] In a first aspect, the present application provides an LED chip, the LED chip comprising:
[0006] substrate;
[0007] An N-type current spreading layer located on one side of the substrate;
[0008] The N-type current spreading layer comprises a first N-type GaN layer, an N-type AlGaN layer and a superlattice structure stacked in a first direction; the superlattice structure comprises a U-type AlGaN layer and a second N-type GaN layer alternately stacked in the first direction; the first direction is perpendicular to the plane where the substrate is located, and points from the substrate to the N-type current spreading layer;
[0009] The doping concentration of the first N-type GaN layer is lower than the doping concentration of the N-type AlGaN layer.
[0010] Preferably, in the above LED chip, the thickness of the first N-type GaN layer ranges from 200 nm to 500 nm, including end points;
[0011] The doping concentration range of the first N-type GaN layer is 2E17 / cm 3 -8E17 / cm 3 , including the endpoint values.
[0012] Preferably, in the above LED chip, the thickness of the N-type AlGaN layer ranges from 300 nm to 800 nm, including end values; the Al component in the N-type AlGaN layer ranges from 0% to 50%;
[0013] The doping concentration range of the N-type AlGaN layer is 2E19 / cm 3 -8E19 / cm 3 , including the endpoint values.
[0014] Preferably, in the above LED chip, the thickness of the U-type AlGaN layer ranges from 2 nm to 8 nm, including end values;
[0015] The Al composition in the U-type AlGaN layer ranges from 0% to 20%.
[0016] Preferably, in the above LED chip, the thickness of the second N-type GaN layer is in the range of 4 nm to 16 nm, including end points.
[0017] Preferably, in the above LED chip, the doping element of the second N-type GaN layer is Si element;
[0018] The doping concentration range of the second N-type GaN layer is 2E18 / cm 3 -9E18 / cm 3 , including the endpoint values.
[0019] Preferably, in the above LED chip, the thickness ratio of the U-type AlGaN layer to the second N-type GaN layer in the superlattice structure is 1:2.
[0020] A second aspect of the present application provides a method for preparing an LED chip, the method for preparing an LED chip comprising:
[0021] providing a substrate;
[0022] An N-type current spreading layer is formed on one side of the substrate; wherein the N-type current spreading layer includes a first N-type GaN layer, an N-type AlGaN layer and a superlattice structure stacked in a first direction; the superlattice structure includes a U-type AlGaN layer and a second N-type GaN layer alternately stacked in the first direction; the first direction is perpendicular to the plane where the substrate is located and points from the substrate to the N-type current spreading layer; the doping concentration of the first N-type GaN layer is lower than the doping concentration of the N-type AlGaN layer.
[0023] Preferably, in the above-mentioned method for preparing the LED chip, the forming of the N-type current spreading layer on one side of the substrate comprises:
[0024] After forming any one of the first N-type GaN layer, the N-type AlGaN layer, the U-type AlGaN layer, and the second N-type GaN layer, surface treatment is performed on the layer.
[0025] A third aspect of the present application provides a light-emitting device, which includes the LED chip described in any one of the above items.
[0026] By means of the above technical scheme, the present application provides an LED chip and its preparation method, and a light-emitting device, wherein the N-type GaN layer in the conventional LED chip is improved to form an N-type current expansion layer, so that it has the function of current expansion. Among them, based on the first N-type GaN layer and the N-type AlGaN layer with gradually increasing doping concentration, the heavily doped N-type AlGaN layer uses the high barrier effect of Al to constrain the flow direction of electrons, promote their lateral expansion, and improve the lateral flow capacity; and by reducing the contact barrier and reducing the high resistance effect through heavy doping, the current congestion phenomenon can be greatly improved, thereby reducing the generation of thermal effects and improving device performance. At the same time, through the interval doping of the U-type AlGaN layer and the second N-type GaN layer, the effective resistivity can be reduced, the longitudinal expansion capacity of the carriers can be improved, and the voltage can be reduced; in addition, the superlattice stress modulation of the U-type AlGaN layer and the second N-type GaN layer can reduce dislocations, which can effectively improve the quality of the crystal, have a great suppression on the reverse leakage of the device, and improve the stability of the LED chip. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The above and other features, advantages and aspects of the embodiments of the present disclosure will become more apparent with reference to the following detailed description in conjunction with the accompanying drawings. Throughout the accompanying drawings, the same or similar reference numerals represent the same or similar elements. It should be understood that the drawings are schematic and the originals and elements are not necessarily drawn to scale.
[0028] Figure 1 A schematic diagram of a partial structure of an LED chip provided by an embodiment of the present invention;
[0029] Figure 2 A schematic diagram of the structure of another LED chip provided by an embodiment of the present invention;
[0030] Figure 3 A schematic diagram of a process for preparing an LED chip provided by an embodiment of the present invention;
[0031] Figure 4 A schematic structural diagram of an LED chip corresponding to a comparative example provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0032] The embodiments of the present application are described below in conjunction with the drawings in the embodiments of the present application. The terms used in the implementation method section of the present application are only used to explain the specific embodiments of the present application, and are not intended to limit the present application. It is known to those of ordinary skill in the art that with the development of technology and the emergence of new scenarios, the technical solutions provided in the embodiments of the present application are also applicable to similar technical problems. It should be noted that the directional words appearing in the present invention are based on the relative position relationship shown in the drawings and cannot be used as an absolute limitation on the present application.
[0033] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0034] refer to Figure 1 , Figure 1 A partial structural diagram of an LED chip provided by an embodiment of the present invention. The LED chip provided by an embodiment of the present invention comprises: a substrate 11, which includes but is not limited to a Si substrate, a PSS sapphire substrate or a SiC substrate.
[0035] An N-type current spreading layer 12 is located on one side of the substrate 11 .
[0036] The N-type current spreading layer 12 includes a first N-type GaN layer 13, an N-type AlGaN layer 14 and a superlattice structure stacked in a first direction; the superlattice structure includes a U-type AlGaN layer 15 and a second N-type GaN layer 16 alternately stacked in the first direction; the first direction is perpendicular to the plane where the substrate 11 is located, and points from the substrate 11 to the N-type current spreading layer 12. The doping concentration of the first N-type GaN layer 13 is lower than the doping concentration of the N-type AlGaN layer 14.
[0037] Specifically, in the embodiment of the present invention, the doping concentration of the first N-type GaN layer 13 is lower than the doping concentration of the N-type AlGaN layer 14, which can be understood as the first N-type GaN layer 13 and the N-type AlGaN layer 14 are prepared by gradient doping, wherein the first N-type GaN layer 13 can be understood as a low-doped film layer or a lightly doped film layer, and the N-type AlGaN layer 14 can be understood as a highly doped film layer or a heavily doped film layer.
[0038] The U-type AlGaN layer 15 represents an intrinsic type of AlGaN layer, that is, the U-type AlGaN layer 15 can be understood as a film layer without any doping. The second N-type GaN layer 16 is N-type doped. Obviously, the superlattice structure formed by the U-type AlGaN layer 15 and the second N-type GaN layer 16 can be understood as a superlattice structure formed by periodic interval doping.
[0039] Specifically, the N-type GaN layer in the conventional LED chip is improved to form an N-type current expansion layer 12, so that it has the function of current expansion. Among them, based on the first N-type GaN layer 13 and the N-type AlGaN layer 14 with gradually increasing doping concentration, the heavily doped N-type AlGaN layer 14 uses the high barrier effect of Al to constrain the flow direction of electrons, promote their lateral expansion, and improve the lateral flow ability; and by reducing the contact barrier and reducing the high resistance effect through heavy doping, the current congestion phenomenon can be greatly improved, thereby reducing the generation of thermal effects and improving device performance. At the same time, through the interval doping of the U-type AlGaN layer 15 and the second N-type GaN layer 16, the effective resistivity can be reduced, the longitudinal expansion ability of the carriers can be improved, and the voltage can be reduced; in addition, the superlattice stress modulation of the U-type AlGaN layer 15 and the second N-type GaN layer 16 can reduce dislocations, which can effectively improve the quality of the crystal, have a great suppression of the reverse leakage of the device, and improve the stability of the LED chip.
[0040] In other words, the LED chip provided by the embodiment of the present invention improves the doping of the interface by designing gradual doping and periodic interval doping, reduces the contact resistance between materials, thereby improving the current expansion capability of the LED chip, reducing the local thermal effect inside the device caused by current crowding, and improving the light efficiency of the LED chip. By optimizing the design of the superlattice layer structure composed of the U-type AlGaN layer 15 and the second N-type GaN layer 16, the superlattice structure formed by periodic interval doping can reduce the effective resistivity, thereby reducing the voltage; and the superlattice stress modulation of the U-type AlGaN layer 15 and the second N-type GaN layer 16 can reduce dislocations, which can effectively improve the quality of the crystal, greatly inhibit the reverse leakage of the device, and improve the stability of the LED chip. The N-type current expansion layer grown under optimized conditions can greatly improve the output light power and antistatic ability of the InGaN / GaN-based LED chip.
[0041] In an optional embodiment of the present invention, reference Figure 2 , Figure 2 A schematic diagram of the structure of another LED chip provided by an embodiment of the present invention. The LED chip provided by an embodiment of the present invention also includes:
[0042] An AlN buffer layer 17 , a three-dimensional nucleation layer 18 and a two-dimensional merged layer 19 are located between the substrate 11 and the N-type current spreading layer 12 and are sequentially stacked in the first direction.
[0043] A low-temperature GaN layer 20, a stress buffer layer 21, a quantum well active layer 22, a P-type AlGaN layer 23 and a P-type GaN layer 24 are located on the side of the N-type current spreading layer 12 away from the substrate 11 and are sequentially stacked in the first direction.
[0044] Specifically, in the embodiment of the present invention, the three-dimensional nucleation layer 18 may also be referred to as a 3D nucleation layer in the art, and the two-dimensional merging layer 19 may also be referred to as a 2D merging layer in the art.
[0045] In an optional embodiment of the present invention, the thickness of the first N-type GaN layer 13 is in the range of 200 nm to 500 nm, including the end value. The doping concentration of the first N-type GaN layer 13 is in the range of 2E17 / cm 3 -8E17 / cm 3 , including the endpoint values.
[0046] Specifically, in the embodiment of the present invention, the main function of the first N-type GaN layer 13 is to repair the rough surface of the three-dimensional nucleation layer 18 after growth, so as to reduce defect density and stress and improve the photoelectric performance of the LED chip.
[0047] In an optional embodiment of the present invention, the thickness of the N-type AlGaN layer 14 is in the range of 300nm-800nm, including the end value. The Al composition of the N-type AlGaN layer 14 is in the range of 0%-50%. The doping concentration of the N-type AlGaN layer is in the range of 2E19 / cm 3 -8E19 / cm 3 , including the endpoint values.
[0048] Specifically, in the embodiment of the present invention, the main function of the N-type AlGaN layer 14 is to provide electrons and improve the lateral expansion capability of carriers.
[0049] In an optional embodiment of the present invention, the thickness of the U-type AlGaN layer 15 is in the range of 2 nm to 8 nm, including end values, and the Al composition in the U-type AlGaN layer 15 is in the range of 0% to 20%.
[0050] The thickness of the second N-type GaN layer 16 is in the range of 4 nm to 16 nm, including the end value. The doping element of the second N-type GaN layer 16 is Si element. The doping concentration of the second N-type GaN layer 16 is in the range of 2E18 / cm 3 -9E18 / cm 3 , including endpoint values. The thickness ratio of the U-type AlGaN layer 15 to the second N-type GaN layer 16 in the superlattice structure is 1:2.
[0051] Specifically, in the embodiment of the present invention, the number of growth cycles of the superlattice structure composed of the U-type AlGaN layer 15 and the second N-type GaN layer 16 can be 20-40, including the end value. The main function of the superlattice structure composed of the U-type AlGaN layer 15 and the second N-type GaN layer 16 is to improve the conductivity of the material and the longitudinal migration ability of the carrier, reduce the voltage, and release the stress of the later grown quantum well active layer.
[0052] Based on the above embodiment of the present invention, another embodiment of the present invention further provides a method for preparing an LED chip, referring to Figure 3 , Figure 3 A schematic flow chart of a method for preparing an LED chip provided in an embodiment of the present invention. The method for preparing an LED chip provided in an embodiment of the present invention comprises:
[0053] S101: providing a substrate 11.
[0054] S102: An N-type current spreading layer 12 is formed on one side of the substrate 11; wherein the N-type current spreading layer 12 includes a first N-type GaN layer 13, an N-type AlGaN layer 14 and a superlattice structure stacked in a first direction; the superlattice structure includes a U-type AlGaN layer 15 and a second N-type GaN layer 16 alternately stacked in the first direction; the first direction is perpendicular to the plane where the substrate 11 is located, and points from the substrate 11 to the N-type current spreading layer 12; the doping concentration of the first N-type GaN layer 13 is lower than the doping concentration of the N-type AlGaN layer 14.
[0055] It should be noted that in the embodiment of the present invention, after forming any one of the first N-type GaN layer 13 , the N-type AlGaN layer 14 , the U-type AlGaN layer 15 , and the second N-type GaN layer 16 , the surface of the layer is treated.
[0056] Exemplarily, H2 / NH3 or H2 / NH3 mixed gas is introduced for surface treatment to repair the surface flatness, and the treatment time range may be 10s-60s, including the end value, to reduce defect density and stress.
[0057] The following is a detailed description of the technical solution of the present application and the technical effects it can achieve by comparison. The main difference between the comparative example and the embodiment is that the N-type layer in the comparative example is the N-type GaN layer of a conventional LED chip. The N-type layer in the embodiment is the N-type current spreading layer 12 designed by the technical solution of the present application.
[0058] Comparative Example:
[0059] like Figure 4 As shown, Figure 4 This is a schematic diagram of the structure of an LED chip corresponding to a comparative example provided by an embodiment of the present invention. The specific preparation process steps are as follows:
[0060] Step 1: Use MOCVD equipment, with trimethylgallium TMGa and triethylgallium TEGa as Ga source, ammonia NH3 as N source, trimethylindium TMIn as In source, trimethylaluminum TMAl as Al source, H2 and N2 as carrier gas, N-type and P-type doping sources are silane SiH4 and bis(cyclopentadienyl)magnesium CP2Mg respectively, use sapphire substrate, and graphite disk as substrate carrier.
[0061] Step 2: In an environment of high temperature of 1050° C. (the temperature range may be 900° C.-1150° C., both inclusive), hydrogenation treatment is performed for 5 min to remove impurities, scratches, particles, etc. on the surface of the substrate 11 .
[0062] Step 3: In an environment with a growth temperature of 1000°C (the temperature range may be 900°C-1150°C, including the end value), TMAl, SiH4, NH3, H2, and N2 are introduced to grow an AlN buffer layer 17. The thickness of the AlN buffer layer 17 ranges from 5nm to 50nm, including the end value, and an AlN buffer layer 17 of 25nm is grown exemplarily. The molar ratio of Si to Al is 0.2 (the molar ratio range may be 0.05-0.5, including the end value).
[0063] Step 4: Grow a three-dimensional nucleation layer 18, introduce NH3, H2, and N2, the growth temperature is 900°C (the temperature range can be 800°C-1000°C, including the end value), the NH3 component is 20% (the NH3 component range can be 30%-80%, including the end value). The growth time is 1 minute (the time range can be 0.5 minutes-3 minutes, including the end value), and the lattice mismatch between GaN and AlN is used as the driving force. In a small ammonia atmosphere, the three-dimensional island growth mode is realized by deposition decomposition.
[0064] Step 5: Grow the two-dimensional merged layer 19, introduce NH3, H2, and N2, the growth temperature is 1100°C (the temperature range can be 900°C-1200°C, including the endpoint value), the NH3 component is 80% (the NH3 component range can be 70%-100%, including the endpoint value). The growth time is 2 minutes (the time range can be 0.5 minutes-3 minutes, including the endpoint value). In a high-temperature and high-ammonia atmosphere, the lateral growth mode is realized by diffusion, and the three-dimensional island-shaped GaN plane is merged to reduce the dislocation density.
[0065] Step 6: Grow an N-type GaN layer 25, introduce TMGa, SiH4, NH3, H2, and N2, grow a thickness of 2000nm (the thickness range can be 1500nm-2500nm, including the end value), grow at a temperature of 1050℃ (the temperature range can be 900℃-1200℃, including the end value), and SiH4 concentration is 2E18 / cm 3 .
[0066] Step 7: grow a low-temperature gallium nitride layer 20, introduce TMGa, NH3, and N2, grow a thickness of 200nm (the thickness range can be 150nm-250nm, including the endpoint value), and a growth temperature of 650°C (the temperature range can be 600°C-800°C, including the endpoint value), and transform the dislocation density into V-shaped pits.
[0067] Step 8: Grow a stress buffer layer 21, introduce TEGa, TMIn, NH3, H2, and N2, and grow 30 cycles (the number of growth cycles can range from 25 to 35, including the endpoint value) of 5nm InGaN / 2nm GaN superlattice with a total thickness of 210nm (the thickness can range from 150nm to 250nm, including the endpoint value), wherein the growth temperature of the well layer is 800℃ (the temperature range can be 700℃-850℃, including the endpoint value), and the growth temperature of the barrier layer is 880℃ (the temperature range can be 800℃-1000℃, including the endpoint value).
[0068] Step 9: grow the quantum well active layer 22, pass TEGa, TMIn, SiH4, NH3, H2, N2, the thickness of the well layer is 3nm, the thickness of the barrier layer is 11nm, and the total thickness is 14nm (the thickness range can be 10nm-16nm, including the end value), wherein the growth temperature of the well layer is 780℃ (the temperature range can be 700℃-850℃, including the end value), the growth temperature of the barrier layer is 900℃ (the temperature range can be 800℃-1000℃, including the end value), and the number of growth cycles of the well layer and the barrier layer is 7 (the number of growth cycles can range from 3 to 9, including the end value). It should be noted that H2 is not passed when growing the well layer, and Si is doped when growing the barrier layer.
[0069] Step 11: Grow a P-type AlGaN layer 23 by introducing TMAl, TMGa, CP2Mg, NH3, and H2, with a thickness of 200 nm (the thickness range can be 150 nm-250 nm, including the end value), in an N2 atmosphere, with a growth pressure of 100 torr, a growth temperature of 900°C (the temperature range can be 850°C-1050°C, including the end value), a growth rate of 20 angstroms / s, and a Mg doping concentration of 5E19 / cm 3 , the Al component is 20% (the Al component range can be 0%-50%, including endpoint values).
[0070] Step 12: Grow a P-type GaN layer 24, introduce TMGa, CP2Mg, NH3, H2, N2, grow a thickness of 400nm (thickness range can be 200nm-600nm, including the end value), grow a temperature of 1050℃ (temperature range can be 800℃-1200℃, including the end value), and a Mg concentration of 1E20 / cm 3 (Mg concentration range can be 1E19 / cm 3 -4E20 / cm 3 , including the endpoint values).
[0071] Step 13: Perform cooling annealing to terminate the growth. Test the epitaxial wafer and make chips, and perform photoelectric parameter testing through EL.
[0072] In the comparative example, the N-type layer is the N-type GaN layer 25 of a conventional LED chip, which has a simple structural design and fixed doping, which easily leads to uneven doping and thus forms a local high resistance phenomenon, resulting in the inability of the current to expand laterally, causing current congestion to form a thermal effect, resulting in low luminous efficiency; and it is easy to form a leakage channel, which can easily cause the LED to die under high current density applications.
[0073] Example:
[0074] like Figure 2 The specific preparation process steps are as follows:
[0075] Step 1: Use MOCVD equipment, with trimethylgallium TMGa and triethylgallium TEGa as Ga source, ammonia NH3 as N source, trimethylindium TMIn as In source, trimethylaluminum TMAl as Al source, H2 and N2 as carrier gas, N-type and P-type doping sources are silane SiH4 and bis(cyclopentadienyl)magnesium CP2Mg respectively, use sapphire substrate, and graphite disk as substrate carrier.
[0076] Step 2: In an environment of high temperature of 1050° C. (the temperature range may be 900° C.-1150° C., both inclusive), hydrogenation treatment is performed for 5 min to remove impurities, scratches, particles, etc. on the surface of the substrate 11 .
[0077] Step 3: In an environment with a growth temperature of 1000°C (the temperature range may be 900°C-1150°C, including the end value), TMAl, SiH4, NH3, H2, and N2 are introduced to grow an AlN buffer layer 17. The thickness of the AlN buffer layer 17 ranges from 5nm to 50nm, including the end value, and an AlN buffer layer 17 of 25nm is grown exemplarily. The molar ratio of Si to Al is 0.2 (the molar ratio range may be 0.05-0.5, including the end value).
[0078] Step 4: Grow a three-dimensional nucleation layer 18, introduce NH3, H2, and N2, the growth temperature is 900°C (the temperature range can be 800°C-1000°C, including the end value), the NH3 component is 20% (the NH3 component range can be 30%-80%, including the end value). The growth time is 1 minute (the time range can be 0.5 minutes-3 minutes, including the end value), and the lattice mismatch between GaN and AlN is used as the driving force. In a small ammonia atmosphere, the three-dimensional island growth mode is realized by deposition decomposition.
[0079] Step 5: Grow the two-dimensional merged layer 19, introduce NH3, H2, and N2, the growth temperature is 1100°C (the temperature range can be 900°C-1200°C, including the endpoint value), the NH3 component is 80% (the NH3 component range can be 70%-100%, including the endpoint value). The growth time is 2 minutes (the time range can be 0.5 minutes-3 minutes, including the endpoint value). In a high-temperature and high-ammonia atmosphere, the lateral growth mode is realized by diffusion, and the three-dimensional island-shaped GaN plane is merged to reduce the dislocation density.
[0080] Step 6: Grow the N-type current spreading layer 12 designed by the technical solution of the present application, introduce TMGa, SiH4, TMAl, NH3, H2, and N2, first grow the first low-doped N-type GaN layer 13, the growth thickness is 300nm (the thickness range can be 200nm-500nm, including the end value), the growth temperature is 1000℃ (the temperature range can be 900℃-1100℃, including the end value), and the concentration of SiH4 is 5E17 / cm 3 .
[0081] All MO sources are turned off, H2 / NH3 or H2 / NH3 mixed gas is introduced, the growth temperature is 1050°C (the temperature range can be 1000°C-1100°C, including the endpoint value), and the growth time is 30s (the growth time range can be 10s-60s, including the endpoint value).
[0082] Then, a highly doped N-type AlGaN layer 14 is grown with a thickness of 500 nm (the thickness range may be 300 nm-800 nm, including the end value), a growth temperature of 1080°C (the temperature range may be 1000°C-1200°C, including the end value), and a SiH4 concentration of 2E19 / cm 3 , the Al component is 30% (the Al component range can be 0%-50%).
[0083] All MO sources are turned off, H2 / NH3 or H2 / NH3 mixed gas is introduced, the temperature is 1100°C (the temperature range can be 1050°C-1150°C, including the endpoint value), and the growth time is 30s (the growth time range can be 10s-60s, including the endpoint value).
[0084] Finally, a superlattice structure consisting of a U-type AlGaN layer 15 and a second N-type GaN layer 16 is grown, wherein the thickness of the U-type AlGaN layer 15 / the second N-type GaN layer 16 is 5nm / 10nm, the Al component in the U-type AlGaN layer 15 is 10% (the Al component range can be 0%-20%), the number of growth cycles is 30 (the number of growth cycles range can be 20-40, including the end value), the U-type AlGaN layer 15 is not doped with Si, and the Si doping concentration in the second N-type GaN layer 16 is 5E18 / cm 3 , growth temperature 1050°C (the temperature range can be 1000°C-1100°C, including endpoint values).
[0085] Step 7: grow a low-temperature gallium nitride layer 20, introduce TMGa, NH3, and N2, grow a thickness of 200nm (the thickness range can be 150nm-250nm, including the endpoint value), and a growth temperature of 650°C (the temperature range can be 600°C-800°C, including the endpoint value), and transform the dislocation density into V-shaped pits.
[0086] Step 8: Grow a stress buffer layer 21, introduce TEGa, TMIn, NH3, H2, and N2, and grow 30 cycles (the number of growth cycles can range from 25 to 35, including the endpoint value) of 5nm InGaN / 2nm GaN superlattice with a total thickness of 210nm (the thickness can range from 150nm to 250nm, including the endpoint value), wherein the growth temperature of the well layer is 800℃ (the temperature range can be 700℃-850℃, including the endpoint value), and the growth temperature of the barrier layer is 880℃ (the temperature range can be 800℃-1000℃, including the endpoint value).
[0087] Step 9: grow the quantum well active layer 22, pass TEGa, TMIn, SiH4, NH3, H2, N2, the thickness of the well layer is 3nm, the thickness of the barrier layer is 11nm, and the total thickness is 14nm (the thickness range can be 10nm-16nm, including the end value), wherein the growth temperature of the well layer is 780℃ (the temperature range can be 700℃-850℃, including the end value), the growth temperature of the barrier layer is 900℃ (the temperature range can be 800℃-1000℃, including the end value), and the number of growth cycles of the well layer and the barrier layer is 7 (the number of growth cycles can range from 3 to 9, including the end value). It should be noted that H2 is not passed when growing the well layer, and Si is doped when growing the barrier layer.
[0088] Step 11: Grow a P-type AlGaN layer 23 by introducing TMAl, TMGa, CP2Mg, NH3, and H2, with a thickness of 200 nm (the thickness range can be 150 nm-250 nm, including the end value), in an N2 atmosphere, with a growth pressure of 100 torr, a growth temperature of 900°C (the temperature range can be 850°C-1050°C, including the end value), a growth rate of 20 angstroms / s, and a Mg doping concentration of 5E19 / cm 3 , the Al component is 20% (the Al component range can be 0%-50%, including endpoint values).
[0089] Step 12: Grow a P-type GaN layer 24, introduce TMGa, CP2Mg, NH3, H2, N2, grow a thickness of 400nm (thickness range can be 200nm-600nm, including the end value), grow a temperature of 1050℃ (temperature range can be 800℃-1200℃, including the end value), and a Mg concentration of 1E20 / cm 3 (Mg concentration range can be 1E19 / cm 3 -4E20 / cm 3 , including the endpoint values).
[0090] Step 13: Perform cooling annealing to terminate the growth. Test the epitaxial wafer and make chips, and perform photoelectric parameter testing through EL.
[0091] The LED chip provided by the embodiment of the present invention improves the doping of the interface by designing gradual doping and periodic interval doping, reduces the contact resistance between materials, thereby improving the current expansion capability of the LED chip, reducing the local thermal effect inside the device caused by current crowding, and improving the light efficiency of the LED chip. By optimizing the design of the superlattice layer structure composed of the U-type AlGaN layer 15 and the second N-type GaN layer 16, the superlattice structure formed by periodic interval doping can reduce the effective resistivity, thereby reducing the voltage; and the superlattice stress modulation of the U-type AlGaN layer 15 and the second N-type GaN layer 16 can reduce dislocations, which can effectively improve the quality of the crystal, greatly suppress the reverse leakage of the device, and improve the stability of the LED chip. The N-type current expansion layer grown under optimized conditions can greatly improve the output light power and antistatic ability of the InGaN / GaN-based LED chip.
[0092] In other words, improving the current expansion capability of InGaN / GaN-based LED chips is an important way to improve the droop effect of LED chips and improve the anti-static ability of LED chips. The conductive properties of N-type GaN play an important role in the uniform expansion of current. The LED chip provided in the embodiment of the present invention improves the current expansion capability of the LED chip by designing a superlattice structure of a first N-type GaN layer 13 and an N-type AlGaN layer 14 with gradual doping, and a periodically doped U-type AlGaN layer 15 and a second N-type GaN layer 16, so that the droop effect of the LED is significantly improved, and the leakage and anti-static capabilities of the LED are also improved.
[0093] Based on the above-mentioned embodiment of the present invention, a light-emitting device is provided in another embodiment of the present invention. The light-emitting device includes the LED chip provided in the embodiment of the present invention.
[0094] The above is a detailed introduction to an LED chip and its preparation method and light-emitting device provided by the present invention. Specific examples are used in this article to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. At the same time, for general technicians in this field, according to the idea of the present invention, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present invention.
[0095] It should be noted that each embodiment in this specification is described in a progressive manner, and each embodiment focuses on the differences from other embodiments, and the same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part description.
[0096] It should also be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or device that includes a series of elements is inherent to the elements, or also includes elements inherent to these processes, methods, articles or devices. In the absence of further restrictions, the elements defined by the sentence "including a..." do not exclude the presence of other identical elements in the process, method, article or device that includes the elements.
[0097] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. An LED chip, It is characterized in that The LED chip comprises: substrate; An N-type current spreading layer located on one side of the substrate; The N-type current spreading layer comprises a first N-type GaN layer, an N-type AlGaN layer and a superlattice structure stacked in a first direction; the superlattice structure comprises a U-type AlGaN layer and a second N-type GaN layer alternately stacked in the first direction; the first direction is perpendicular to the plane where the substrate is located, and points from the substrate to the N-type current spreading layer; The doping concentration of the first N-type GaN layer is lower than the doping concentration of the N-type AlGaN layer.
2. The LED chip according to claim 1, It is characterized in that The thickness of the first N-type GaN layer is in the range of 200 nm to 500 nm, including end points; The doping concentration range of the first N-type GaN layer is 2E17 / cm 3 -8E17 / cm 3 , including the endpoint values.
3. The LED chip according to claim 1, It is characterized in that The thickness of the N-type AlGaN layer ranges from 300 nm to 800 nm, including end values; the Al composition in the N-type AlGaN layer ranges from 0% to 50%; The doping concentration range of the N-type AlGaN layer is 2E19 / cm 3 -8E19 / cm 3 , including the endpoint values.
4. The LED chip according to claim 1, It is characterized in that The thickness of the U-type AlGaN layer is in the range of 2 nm to 8 nm, including end values; The Al composition in the U-type AlGaN layer ranges from 0% to 20%.
5. The LED chip according to claim 1, It is characterized in that The thickness of the second N-type GaN layer is in a range of 4 nm to 16 nm, including end points.
6. The LED chip according to claim 1, It is characterized in that The doping element of the second N-type GaN layer is Si element; The doping concentration range of the second N-type GaN layer is 2E18 / cm 3 -9E18 / cm 3 , including the endpoint values.
7. The LED chip according to any one of claims 1 to 6, It is characterized in that The thickness ratio of the U-type AlGaN layer to the second N-type GaN layer in the superlattice structure is 1:
2.
8. A method for preparing an LED chip, It is characterized in that The method for preparing the LED chip comprises: providing a substrate; An N-type current spreading layer is formed on one side of the substrate; wherein the N-type current spreading layer includes a first N-type GaN layer, an N-type AlGaN layer and a superlattice structure stacked in a first direction; the superlattice structure includes a U-type AlGaN layer and a second N-type GaN layer alternately stacked in the first direction; the first direction is perpendicular to the plane where the substrate is located and points from the substrate to the N-type current spreading layer; the doping concentration of the first N-type GaN layer is lower than the doping concentration of the N-type AlGaN layer.
9. The method for preparing an LED chip according to claim 8, It is characterized in that The forming of an N-type current spreading layer on one side of the substrate comprises: After forming any one of the first N-type GaN layer, the N-type AlGaN layer, the U-type AlGaN layer, and the second N-type GaN layer, surface treatment is performed on the layer.
10. A light emitting device, It is characterized in that The light emitting device comprises the LED chip according to any one of claims 1-7.
Citation Information
Cited By
Epitaxial structure, power device and manufacturing method of epitaxial structure
TWI937646B