High-specific-capacity graphite negative electrode composite material and preparation method thereof
Through chemical vapor deposition and vapor coating technology, silica/carbon nanotube/graphite negative electrode composite materials were prepared, which solved the problems of low specific capacity and poor cycle stability of graphite negative electrode materials, and achieved the effect of high specific capacity and long life , suitable for the industrial application of lithium-ion batteries.
Patent Information
- Application Number
- CN202411145518.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-29
AI Technical Summary
The existing graphite negative electrode materials have low specific capacity and poor cycle stability, which limit the service life and industrial application of lithium-ion batteries.
The silica @ carbon nanotube and the vapor-coated graphite material are prepared by chemical vapor deposition, and combined with a binder to form a silica/carbon nanotube/graphite negative electrode composite material to improve the specific capacity and cycle stability of the material.
It significantly improves the capacitance and service life, is suitable for large-scale industrial applications, and enhances the conductivity and cyclic stability of composite materials.
Smart Images

Figure BDA0005002087620000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of negative electrode composite materials, and in particular to a high specific capacity graphite negative electrode composite material and a preparation method thereof. Background Art
[0002] In recent years, the rapid growth of the lithium-ion power battery market has put forward higher requirements on the performance of high-capacity negative electrode materials. As one of the important indicators, the service life of lithium-ion batteries is not only of extraordinary significance in alleviating the problems of battery life and charging, but also can promote energy conservation, emission reduction and environmental protection.
[0003] The mainstream negative electrode active materials of lithium-ion batteries are graphitized carbon materials, such as artificial graphite and natural graphite. This is because the low electronic conductivity of the composite and the volume expansion and contraction during the charge and discharge process seriously affect the rate performance and cycle stability of the graphite composite material itself. Although graphite is a relatively mature negative electrode material currently in use, it still has disadvantages such as low negative electrode specific capacity; and at the same time, there are problems such as complex production process and poor cycle stability of the obtained negative electrode material, which is not conducive to the large-scale industrial application of this material. Summary of the invention
[0004] In order to solve the above technical problems, the purpose of the present invention is to provide a high specific capacity graphite negative electrode composite material and a preparation method thereof, wherein silicon dioxide @ carbon nanotubes are obtained by chemical vapor deposition, and a graphite material and a binder after gas phase coating are prepared to obtain a silicon dioxide / carbon nanotube / graphite negative electrode composite material, which effectively solves the problems of low specific capacity of the negative electrode and poor cycle stability in the prior art.
[0005] The technical solution of the present invention to solve the above technical problems is as follows: a method for preparing a high specific capacity graphite negative electrode composite material is provided, comprising the following steps:
[0006] (1) grinding and mixing silica and a catalyst, placing them in a quartz boat, and then placing them in an argon environment, heating, introducing a carbon source and nitrogen mixed gas for chemical vapor deposition while pressurizing to keep the pressure constant, cooling to room temperature after the reaction, crushing, and sieving to obtain silica@carbon nanotubes;
[0007] (2) oxidizing and intercalating spherical graphite with concentrated sulfuric acid and potassium permanganate, and then expanding the spherical graphite to obtain micro-expanded graphite; and then gas-coating the micro-expanded graphite in a mixed gas of methane and nitrogen to obtain a graphite material;
[0008] (3) The silicon dioxide@carbon nanotubes obtained in step (1) are mixed with a surfactant, and then the graphite material and the binder obtained in step (2) are added and mixed evenly, and then coated on the surface of the current collector, dried and then heated in vacuum to obtain a high specific capacity graphite negative electrode composite material.
[0009] Furthermore, in step (1), the mass ratio of silicon dioxide to catalyst is 95-98:2-5.
[0010] Furthermore, in step (1), the catalyst is at least one of ferric nitrate, cobalt nitrate and nickel nitrate.
[0011] Furthermore, in step (1), heating is performed to 600-800°C.
[0012] Furthermore, in step (1), the carbon source gas flow rate is 40-60 sccm, and the nitrogen gas flow rate is 80-120 sccm.
[0013] Furthermore, in step (1), the carbon source is at least one of methane, ethylene, propylene and propane.
[0014] Furthermore, in step (1), chemical vapor deposition is performed at a temperature of 800-1000° C. for 4-6 hours.
[0015] Furthermore, in step (1), the pressure is 5-8 kPa.
[0016] Furthermore, in step (2), the mass ratio of concentrated sulfuric acid, potassium permanganate and spherical graphite is 2-4:0.1-0.2:0.5-1.
[0017] Furthermore, in step (2), the expansion treatment is performed at 1000-1200° C. for 0.2-1 min.
[0018] Furthermore, in step (2), the expansion volume of the micro-expanded graphite is 8-10 mL / g.
[0019] Furthermore, in step (2), the volume ratio of methane to nitrogen is 1:5-20, and the flow rate of the mixed gas is 50-150 sccm.
[0020] Furthermore, in step (2), the gas phase coating is carried out in a fluidized bed at 800-1200° C. and 2-4 kPa for 1-3 hours.
[0021] Furthermore, in step (2), the concentration of concentrated sulfuric acid is 95-98 vt%.
[0022] Furthermore, in step (3), the mass ratio of silicon dioxide@carbon nanotubes, surfactant, graphite material and binder is 10:30-50:5-40:0.1-1.
[0023] Furthermore, in step (3), the surfactant is sodium dodecylbenzene sulfonate or polyvinyl pyrrolidone.
[0024] Furthermore, in step (3), the binder is polyvinyl chloride and / or polystyrene.
[0025] Furthermore, in step (3), drying is performed at 70-90° C., and vacuum heating is performed at 100-200° C. for 0.5-3 h.
[0026] The present invention has the following beneficial effects:
[0027] 1. The present invention obtains silicon dioxide @ carbon nanotubes by chemical vapor deposition, and prepares silicon dioxide / carbon nanotube / graphite negative electrode composite materials with gas-coated graphite materials and binders, which effectively solves the problems of low negative electrode specific capacity and poor cycle stability in the prior art; the obtained composite material has large capacitance and long service life, can greatly improve the production efficiency of the material, and is suitable for large-scale industrial application of the material.
[0028] 2. During the preparation, silicon dioxide and catalyst are heated and then introduced into a mixed gas, and carbon nanotubes are synthesized in the process of vapor deposition. The catalyst is used to catalyze the formation of carbon nanotubes in the process of chemical vapor deposition. Then, concentrated sulfuric acid and potassium permanganate are used to oxidize and intercalate the spherical graphite, and then a mixed gas of methane and nitrogen is introduced for gas phase coating. More gas molecules diffuse into the gaps and cracks in the spherical micro-expanded graphite to fill the pores and cracks, which can improve the structural defects of the graphite itself and improve the specific capacity and cycle stability of the material. After mixing silicon dioxide @ carbon nanotubes with surfactants, graphite materials and binders are added and mixed, and after coating and treatment, silicon dioxide / carbon nanotubes / graphite negative electrode composite materials are obtained; the graphite material after gas phase coating is used to coat silicon dioxide @ carbon nanotubes to form a composite material, which enhances the conductivity between the particles inside the composite material, improves the specific capacity, and the addition of silicon dioxide @ carbon nanotubes also improves its cycle stability. DETAILED DESCRIPTION
[0029] The principles and features of the present invention are described below, and the examples are only used to explain the present invention and are not used to limit the scope of the present invention. If no specific conditions are specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.
[0030] Example 1
[0031] A high specific capacity graphite negative electrode composite material, the preparation method of which comprises the following steps:
[0032] (1) Grinding and mixing silica and a catalyst, placing them in a quartz boat, and then placing them in an argon environment, heating them to 600°C, introducing a carbon source and a nitrogen mixture gas, and chemically vapor depositing them at 800°C for 4 hours, while pressurizing them to 5 kPa to keep the pressure constant, cooling them to room temperature after the reaction, crushing them, and sieving them to obtain silica@carbon nanotubes; the mass ratio of silica to catalyst (ferric nitrate) was 95:5; the carbon source (methane) gas flow rate was 40 sccm, and the nitrogen gas flow rate was 80 sccm;
[0033] (2) 95vt% concentrated sulfuric acid and potassium permanganate were used to oxidize and intercalate spherical graphite, and then expanded at 1000°C for 0.5 min to obtain slightly expanded graphite; the slightly expanded graphite was then gas-coated in a mixed gas of methane and nitrogen in a fluidized bed at 800°C and 2kPa for 1 h to obtain a graphite material; the mass ratio of concentrated sulfuric acid, potassium permanganate and spherical graphite was 2:0.1:0.5; the volume ratio of methane to nitrogen was 1:5, and the gas flow rate of the mixed gas was 50sccm;
[0034] (3) The silica@carbon nanotubes obtained in step (1) are mixed with a surfactant (polyvinyl pyrrolidone), and then the graphite material and binder (polyvinyl chloride) obtained in step (2) are added and mixed evenly, coated on the surface of the current collector, dried at 70°C, and vacuum heated at 100°C for 0.5h to obtain a high specific capacity graphite negative electrode composite material; the mass ratio of silica@carbon nanotubes, surfactant, graphite material and binder is 10:30:5:0.2.
[0035] Example 2
[0036] A high specific capacity graphite negative electrode composite material, the preparation method of which comprises the following steps:
[0037] (1) Grinding and mixing silica and a catalyst, placing them in a quartz boat, and then placing them in an argon environment, heating them to 700°C, introducing a carbon source and a nitrogen mixture gas, and chemically vapor depositing them at 900°C for 5 hours, while pressurizing them to 6 kPa to keep the pressure constant, cooling them to room temperature after the reaction, crushing them, and sieving them to obtain silica@carbon nanotubes; the mass ratio of silica to catalyst (ferric nitrate) was 96:4; the carbon source (methane) gas flow rate was 50 sccm, and the nitrogen gas flow rate was 100 sccm;
[0038] (2) 96vt% concentrated sulfuric acid and potassium permanganate were used to oxidize and intercalate spherical graphite, and then expanded at 1100°C for 0.5 min to obtain slightly expanded graphite; the slightly expanded graphite was then gas-coated in a mixed gas of methane and nitrogen in a fluidized bed at 1000°C and 3kPa for 2h to obtain a graphite material; the mass ratio of concentrated sulfuric acid, potassium permanganate and spherical graphite was 3:0.2:0.8; the volume ratio of methane to nitrogen was 1:10, and the gas flow rate of the mixed gas was 100sccm;
[0039] (3) The silica@carbon nanotubes obtained in step (1) are mixed with a surfactant (polyvinyl pyrrolidone), and then the graphite material and binder (polyvinyl chloride) obtained in step (2) are added and mixed evenly, coated on the surface of the current collector, dried at 80°C, and vacuum heated at 150°C for 1.5h to obtain a high specific capacity graphite negative electrode composite material; the mass ratio of silica@carbon nanotubes, surfactant, graphite material and binder is 10:40:20:0.5.
[0040] Example 3
[0041] A high specific capacity graphite negative electrode composite material, the preparation method of which comprises the following steps:
[0042] (1) Grinding and mixing silica and a catalyst, placing them in a quartz boat, and then placing them in an argon environment, heating them to 800°C, introducing a carbon source and a nitrogen mixture gas, and chemically vapor depositing them at 1000°C for 6 hours, while pressurizing them to 8 kPa to keep the pressure constant, cooling them to room temperature after the reaction, crushing them, and sieving them to obtain silica@carbon nanotubes; the mass ratio of silica to catalyst (nickel nitrate) was 98:2; the carbon source (propane) gas flow rate was 60 sccm, and the nitrogen gas flow rate was 120 sccm;
[0043] (2) 98vt% concentrated sulfuric acid and potassium permanganate were used to oxidize and intercalate spherical graphite, and then expanded at 1200°C for 1 min to obtain slightly expanded graphite; the slightly expanded graphite was then gas-coated in a mixed gas of methane and nitrogen in a fluidized bed at 1200°C and 4kPa for 3 hours to obtain a graphite material; the mass ratio of concentrated sulfuric acid, potassium permanganate and spherical graphite was 4:0.2:1; the volume ratio of methane to nitrogen was 1:15, and the gas flow rate of the mixed gas was 1150sccm;
[0044] (3) Mixing the silica@carbon nanotubes obtained in step (1) with a surfactant (polyvinyl pyrrolidone), then adding the graphite material and binder (polystyrene) obtained in step (2) and mixing evenly, coating the mixture on the surface of the current collector, drying at 90°C, and heating at 200°C in vacuum for 3h to obtain a high specific capacity graphite negative electrode composite material; the mass ratio of silica@carbon nanotubes, surfactant, graphite material and binder is 10:50:40:1.
[0045] Comparative Example 1
[0046] A graphite negative electrode composite material, the preparation method of which comprises the following steps:
[0047] (1) Spherical graphite is oxidized and intercalated with 96vt% concentrated sulfuric acid and potassium permanganate, and then expanded at 1100°C for 0.5min to obtain slightly expanded graphite; the slightly expanded graphite is then gas-coated in a mixed gas of methane and nitrogen in a fluidized bed at 1000°C and 3kPa for 2h to obtain a graphite material; the mass ratio of concentrated sulfuric acid, potassium permanganate and spherical graphite is 3:0.2:0.8; the volume ratio of methane to nitrogen is 1:10, and the gas flow rate of the mixed gas is 100sccm;
[0048] (2) Mixing silica with a surfactant (polyvinyl pyrrolidone), then adding the graphite material and binder (polyvinyl chloride) obtained in step (1) and mixing evenly, coating the mixture on the surface of the current collector, drying at 80° C., and heating at 150° C. in a vacuum chamber for 1.5 h to obtain a graphite negative electrode composite material; the mass ratio of silica, surfactant, graphite material and binder is 10:40:20:0.5.
[0049] Comparative Example 2
[0050] A graphite negative electrode composite material, the preparation method of which comprises the following steps:
[0051] (1) Grinding and mixing silica and a catalyst, placing them in a quartz boat, and then placing them in an argon environment, heating them to 700°C, introducing a carbon source and a nitrogen mixture gas, and chemically vapor depositing them at 900°C for 5 hours, while pressurizing them to 6 kPa to keep the pressure constant, cooling them to room temperature after the reaction, crushing them, and sieving them to obtain silica@carbon nanotubes; the mass ratio of silica to catalyst (ferric nitrate) was 96:4; the carbon source (methane) gas flow rate was 50 sccm, and the nitrogen gas flow rate was 100 sccm;
[0052] (2) gas-coating graphite in a mixed gas of methane and nitrogen at 1000° C. and 3 kPa in a fluidized bed for 2 h to obtain a graphite material; the volume ratio of methane to nitrogen was 1:10, and the gas flow rate of the mixed gas was 100 sccm;
[0053] (3) The silica@carbon nanotubes obtained in step (1) are mixed with a surfactant (polyvinyl pyrrolidone), and then the graphite material and binder (polyvinyl chloride) obtained in step (2) are added and mixed evenly, coated on the surface of the current collector, dried at 80°C, and vacuum heated at 150°C for 1.5h to obtain a graphite negative electrode composite material; the mass ratio of silica@carbon nanotubes, surfactant, graphite material and binder is 10:40:20:0.5.
[0054] Comparative Example 3
[0055] A graphite negative electrode composite material, the preparation method of which comprises the following steps:
[0056] (1) Spherical graphite is oxidized and intercalated with 96vt% concentrated sulfuric acid and potassium permanganate, and then expanded at 1100°C for 0.5min to obtain slightly expanded graphite; the slightly expanded graphite is then gas-coated in a mixed gas of methane and nitrogen in a fluidized bed at 1000°C and 3kPa for 2h to obtain a graphite material; the mass ratio of concentrated sulfuric acid, potassium permanganate and spherical graphite is 3:0.2:0.8; the volume ratio of methane to nitrogen is 1:10, and the gas flow rate of the mixed gas is 100sccm;
[0057] (2) Mixing silica, carbon nanotubes and a surfactant (polyvinyl pyrrolidone), then adding the graphite material and a binder (polyvinyl chloride) obtained in step (1) and mixing evenly, coating the mixture on the surface of the current collector, drying the mixture at 80° C., and heating the mixture at 150° C. in a vacuum oven for 1.5 h to obtain a graphite negative electrode composite material; the mass ratio of silica@carbon nanotubes, surfactant, graphite material and binder is 10:40:20:0.5.
[0058] The graphite negative electrode composite materials obtained in Examples 1-3 and Comparative Examples 1-3 were respectively used as the negative electrode, the sheet as the counter electrode, Celgard as the separator, the electrolyte EC:DEC:DMC=1:1:1 (w / w) 1 mole LiPF6, assembled into C / Li half-cells, and then the electrochemical specific capacity test was carried out. The results are shown in Table 1.
[0059] Table 1 Electrochemical specific capacity test results
[0060]
[0061] As can be seen from Table 1, the first charge and discharge capacity, first charge and discharge efficiency and 100-week cycle capacity retention rate of the high specific capacity graphite negative electrode composite material obtained by the present invention are significantly higher than those of Comparative Examples 1-3, which shows that in the composite material, both silicon dioxide @ carbon nanotubes and micro-expanded graphite play an important role. Micro-expanded graphite is more convenient for gas molecules to fill pores and cracks during gas phase coating, improves the structural defects of graphite itself, and improves the specific capacity and cycle stability of the composite material; and the introduction of silicon dioxide @ carbon nanotubes, and the use of graphite materials to coat silicon dioxide @ carbon nanotubes to form a composite material, also enhance the conductivity of the composite material, improve the specific capacity and improve the cycle stability. However, if carbon nanotubes are directly added, the above effect cannot be achieved, and it is also necessary to first combine it with silicon dioxide by vapor deposition to form silicon dioxide @ carbon nanotubes and then combine it with graphite materials to achieve the purpose of increasing the specific capacity and improving the cycle stability.
[0062] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a high specific capacity graphite negative electrode composite material, characterized in that: The following steps are involved: (1) grinding and mixing silica and a catalyst, placing them in a quartz boat, and then placing them in an argon environment, heating, introducing a carbon source and nitrogen mixed gas for chemical vapor deposition while pressurizing to keep the pressure constant, cooling to room temperature after the reaction, crushing, and sieving to obtain silica@carbon nanotubes; (2) oxidizing and intercalating spherical graphite with concentrated sulfuric acid and potassium permanganate, and then expanding the spherical graphite to obtain micro-expanded graphite; and then gas-coating the micro-expanded graphite in a mixed gas of methane and nitrogen to obtain a graphite material; (3) The silicon dioxide@carbon nanotubes obtained in step (1) are mixed with a surfactant, and then the graphite material and the binder obtained in step (2) are added and mixed evenly, and then coated on the surface of the current collector, dried and then heated in vacuum to obtain a high specific capacity graphite negative electrode composite material.
2. The method for preparing the high specific capacity graphite negative electrode composite material according to claim 1, characterized in that: In step (1), the mass ratio of silicon dioxide to catalyst is 95-98:2-5.
3. The method for preparing the high specific capacity graphite negative electrode composite material according to claim 1, characterized in that: In step (1), the carbon source is at least one of methane, ethylene, propylene and propane.
4. The method for preparing the high specific capacity graphite negative electrode composite material according to claim 1, characterized in that: In step (1), chemical vapor deposition is carried out at a temperature of 800-1000° C. for 4-6 hours.
5. The method for preparing the high specific capacity graphite negative electrode composite material according to claim 1, characterized in that: In step (2), the mass ratio of concentrated sulfuric acid, potassium permanganate and spherical graphite is 2-4:0.1-0.2:0.5-1.
6. The method for preparing the high specific capacity graphite negative electrode composite material according to claim 1, characterized in that: In step (2), the expansion treatment is performed at 1000-1200° C. for 0.2-1 min.
7. The method for preparing the high specific capacity graphite negative electrode composite material according to claim 1, characterized in that: In step (2), the gas phase coating is carried out in a fluidized bed at 800-1200° C. and 2-4 kPa for 1-3 hours.
8. The method for preparing the high specific capacity graphite negative electrode composite material according to claim 1, characterized in that: In step (3), the mass ratio of silicon dioxide@carbon nanotubes, surfactant, graphite material and binder is 10:30-50:5-40:0.1-1.
9. The method for preparing the high specific capacity graphite negative electrode composite material according to claim 1, characterized in that: In step (3), drying is performed at a temperature of 70-90° C., and vacuum heating is performed at a temperature of 100-200° C. for 0.5-3 h.
10. The high specific capacity graphite negative electrode composite material obtained by the preparation method of the high specific capacity graphite negative electrode composite material according to any one of claims 1 to 9.
Citation Information
Cited By
Fast charging type graphite negative electrode material and preparation method and application thereof
CN122051225A
Fast-charging graphite negative electrode material, preparation method and application thereof
CN122051225B