Anion-cation co-doped lithium-rich manganese-based positive electrode material as well as preparation method and application thereof

Through the preparation of anion-cationic co-doped lithium-rich manganese-based positive electrode material, the spinel phase is formed by hydrothermal reaction between nickel-cobalt-manganese ternary precursor and Na2S·9H2O or NaF, which solves the voltage of existing materials in long-term circulation. The problem of attenuation significantly improves the stability of capacity and voltage.

CN119050340APending Publication Date: 2024-11-29YANGZHOU POLYTECHNIC INST
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411321364.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing lithium-rich manganese-based positive electrode materials have severe voltage attenuation during long-term cycles, resulting in a reduced energy density, which is an urgent technical challenge.

Method used

The preparation method of anion-cationic co-doped lithium-rich manganese-based positive electrode material is adopted. The material structure of the spinel phase is formed by hydrothermal reaction between the nickel-cobalt-manganese ternary precursor and Na2S·9H2O or NaF, and combined with lithiated calcination technology. , a stable lattice framework is formed in situ in the body phase, and anions are uniformly doped to slow down the Li/Ni mixed displacement.

Benefits of technology

A capacity retention rate of up to 100% and voltage retention rate of 92.9% after cycling for 200 cycles at 250 mA g–1 current density is achieved. The average voltage loss per charge and discharge is only 0.99 mV, which significantly improves the cycling performance of the material and Voltage stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050340A_ABST
    Figure CN119050340A_ABST
Patent Text Reader

Abstract

The invention relates to an anion-cation co-doped lithium-rich manganese-based positive electrode material and a preparation method and application thereof, the chemical general formula of the positive electrode material is LiA < 1-w > [Li < 1-x-2y > Ni < x > Co < y > Mn < 2-2x-y / 3 >] O < 2-z > B < z >, A is Na, and B is F or S. The anion-cation co-doped lithium-rich manganese-based positive electrode material is obtained by performing hydrothermal doping on a nickel-cobalt-manganese ternary precursor in advance and then performing lithiation calcination for the first time, and the treatment method can form a spinel phase with higher lattice framework stability in a bulk phase in situ; the spinel structure provides a three-dimensional channel for rapid transmission of lithium ions and relieves migration of transition metal ions in a high-voltage cycle process; the negative ions are uniformly doped in the bulk phase of the material, so that Li / Ni mixed arrangement can be effectively slowed down, and lithium ion transmission is improved; finally, the modified positive electrode material shows good cycle performance and shows excellent capacity stability and voltage stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium batteries, and specifically to a lithium-rich manganese-based cathode material with co-doping of anions and cations, a preparation method thereof, and an application thereof. Background Art

[0002] Developing lithium-ion batteries with higher energy density and longer cycle life remains an important part of sustainable energy technology research. The cathode material determines the performance, safety, and cost of lithium-ion batteries and has always been the core of lithium-ion batteries. Compared with traditional cathode materials, lithium-rich manganese-based cathode materials (xLi2MnO3•(1-x)LiMO2, M = transition metal (TM), 0 < x < 1) have extremely high theoretical specific capacity (>350 mAh g –1 ) and reversible specific capacity (>250 mAh g –1 ), and have become a research hotspot of cathode materials. The electrochemical performance of lithium-rich manganese-based cathode materials is related not only to the single transition metal oxidation mechanism in traditional cathode materials, but also the anion-based redox reaction provides higher capacity. Although the anion charge compensation reaction improves the specific capacity of the material, it also brings many problems, such as voltage decay during long-term cycling, which greatly reduces the energy density of the cathode material and is an urgent problem to be solved. Summary of the Invention

[0003] Aiming at the deficiencies in the prior art, the present invention proposes a lithium-rich manganese-based cathode material with co-doping of anions and cations.

[0004] To achieve the above object, the present invention provides the following technical solutions: A lithium-rich manganese-based cathode material with co-doping of anions and cations, the chemical general formula of the cathode material is LiA 1-w [Li 1-x-2y Ni x Co y Mn 2-2x-y / 3 O 2-z B z , where 0.05 < x ≤ 0.25; 0.05 ≤ y ≤ 0.25; 0.7 ≤ x + 2y ≤ 1; 0 < z ≤ 0.1; 0.9 < w ≤ 1; A is Na, and B is F or S.

[0005] The second object of the present invention provides a preparation method of the above-mentioned lithium-rich manganese-based cathode material with co-doping of anions and cations, including the following steps: 1) A nickel-cobalt-manganese ternary precursor Ni x Co y Mn 2-2x-y / 3 (OH) a, where 0.05<x≤0.25, 0.05≤y≤0.25, 0.7≤x+2y≤1, 1.5≤a≤3, put into an aqueous solution of a compound containing elements A and B, stir to fully dissolve the sample, transfer to a polytetrafluoroethylene reactor for hydrothermal reaction; after the reaction, the sample is cooled and allowed to stand, centrifuged, washed and dried; 2) Grind the treated precursor and lithium carbonate in a mortar, mix thoroughly and pre-sinter, then heat and calcine, and grind thoroughly after cooling in the furnace to obtain anion-cation co-doped lithium-rich manganese-based positive electrode material.

[0006] Furthermore, the compound containing elements A and B is Na2S·9H2O or NaF.

[0007] Furthermore, in the step 1), the mass ratio of the nickel-cobalt-manganese ternary precursor to the compound containing elements A and B is 1:0.5-1.

[0008] Furthermore, in the step 2), the mass ratio of the treated precursor to lithium carbonate is 1:0.66-1.

[0009] Furthermore, in step 2), the pre-calcination heating rate is 2-10 ℃ / min –1 , calcined at 400-600℃ for 4-6h; the calcination heating rate is 5-15℃ / min –1 , calcined at 800-1000℃ for 10-20 h.

[0010] The third object of the present invention is to provide an application of the positive electrode material of the first scheme in a lithium ion battery, which includes the anion-cation co-doped lithium-rich manganese-based positive electrode material as described above.

[0011] Compared with the prior art, the present invention has the following beneficial effects: 1) The present invention is the first to obtain anion-cation co-doped lithium-rich manganese-based positive electrode material by pre-hydrothermal doping of a nickel-cobalt-manganese ternary precursor and then calcining it for lithiumation. This treatment method can form a spinel phase with higher lattice framework stability in situ in the bulk phase; the spinel structure provides a three-dimensional channel for the rapid transmission of lithium ions and alleviates the migration of transition metal ions during high-voltage cycling; 2) The uniform doping of anions in the bulk phase of the material can effectively slow down the Li / Ni mixing and improve the lithium ion transmission. Finally, the modified cathode material shows a high conductivity at 250 mA g –1 The capacity retention rate is as high as 100% after 200 cycles at the same current density, and it also has outstanding voltage stability at 250 mA g –1 The voltage retention rate after 200 cycles at the current density is 92.9%, and the average voltage loss per charge and discharge is only 0.99 mV. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 The electron microscope image and XRD pattern of the positive electrode material prepared in Example 1.

[0013] Figure 2 The figure is a charge and discharge cycle curve diagram of the positive electrode material prepared based on the comparative example and embodiment 1.

[0014] Figure 3 Graph showing the discharge voltage of the positive electrode materials prepared based on the comparative example and Example 1.

[0015] Figure 4 The figure is a charge and discharge cycle curve diagram of the positive electrode material prepared based on the comparative example and embodiment 2.

[0016] Figure 5 Graph showing the discharge voltage of the positive electrode materials prepared based on the comparative example and Example 2.

[0017] Figure 6 The figure is a charge and discharge cycle curve diagram of the positive electrode material prepared based on the comparative example and Example 3.

[0018] Figure 7 Graph showing the discharge voltage of the positive electrode materials prepared based on the comparative example and Example 3. DETAILED DESCRIPTION

[0019] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0021] Embodiment 1: (1) Ni 0.13 Co 0.13 Mn 0.54 The (OH)2 precursor is placed in a certain proportion of Na2S·9H2O aqueous solution, in which Ni 0.13 Co 0.13 Mn 0.54 The mass ratio of (OH)2 precursor and Na2S·9H2O was 1:0.5, and the sample was stirred for 20 min to fully dissolve, and then transferred to a polytetrafluoroethylene reactor for hydrothermal reaction for 2 h at 120°C. The reacted sample was cooled and allowed to stand, then centrifuged, washed with water and ethanol three times to remove unreacted impurities, and then dried in a vacuum drying oven at 80°C overnight; (2) The treated precursor and lithium carbonate were placed in a mortar at a mass ratio of 1:0.66 and manually ground for 1 h. The fully mixed sample was pre-sintered at 600 °C for 5 h, then heated to 900 °C and calcined for 15 h. After cooling in the furnace, it was fully ground to obtain an anion-cation co-doped positive electrode material.

[0022] like Figure 1 As shown, the positive electrode material cations occupy the Li layer, and the anions are evenly dispersed in the bulk phase, occupying the sites of oxygen ions, without changing the valence of other transition metal ions (Ni, Co, Mn), and at the same time forming a spinel phase in situ in the bulk phase, which is a secondary sphere formed by the accumulation of irregular particles of about 350 nm, and the diameter of the secondary particles is about 4.0 μm. In addition to the layered region, the anion-cation co-doped lithium-rich manganese-based positive electrode material also has spinel regions belonging to the Fd-3m space group on the surface and inside of the material.

[0023] Embodiment 2: (1) Ni 0.13 Co 0.13 Mn 0.54 The (OH)2 precursor is placed in a certain proportion of Na2S·9H2O aqueous solution, in which Ni 0.13 Co 0.13 Mn 0.54 The mass ratio of (OH)2 precursor and Na2S·9H2O was 1:0.7, and the sample was stirred for 20 min to fully dissolve, and then transferred to a polytetrafluoroethylene reactor for hydrothermal reaction for 2 h at 120°C. The reacted sample was cooled and allowed to stand, then centrifuged, washed with water and ethanol three times to remove unreacted impurities, and then dried in a vacuum drying oven at 80°C overnight; (2) The treated precursor and lithium carbonate were placed in a mortar at a mass ratio of 1:0.66 and manually ground for 1 h. The fully mixed sample was pre-sintered at 600 °C for 5 h, then heated to 900 °C and calcined for 15 h. After cooling in the furnace, it was fully ground to obtain an anion-cation co-doped positive electrode material.

[0024] Embodiment 3: (1) Ni 0.13 Co 0.13 Mn 0.54 The (OH)2 precursor is placed in a certain proportion of NaF aqueous solution, in which Ni 0.13 Co 0.13 Mn 0.54The mass ratio of (OH)2 precursor and NaF was 1:1, and the sample was stirred for 20 min to fully dissolve, and then transferred to a polytetrafluoroethylene reactor for hydrothermal reaction for 2 h at 120°C. The sample after reaction was cooled and allowed to stand, then centrifuged, washed with water and ethanol three times to remove unreacted impurities, and then dried in a vacuum drying oven at 80°C overnight; (2) The treated precursor and lithium carbonate were placed in a mortar at a mass ratio of 1:0.66 and manually ground for 1 h. The fully mixed sample was pre-sintered at 600 °C for 5 h, then heated to 900 °C and calcined for 15 h. After cooling in the furnace, it was fully ground to obtain an anion-cation co-doped positive electrode material.

[0025] Comparative Example: An Undoped Lithium-Rich Manganese-Based Cathode Material Ni 0.13 Co 0.13 Mn 0.54 The (OH)2 precursor and Li2CO3 were put into a mortar and ground manually for 1 h at a mass ratio of 1:0.66. The fully mixed sample was pre-sintered at 600 °C for 5 h, then heated to 900 °C for 15 h, and fully ground after cooling in the furnace to obtain the undoped lithium-rich manganese-based positive electrode material Li 1.2 Ni 0.13 Co 0.13 Mn 0.54 O2.

[0026] test: Assembly and testing of button cells: positive electrode material, carbon black conductive agent, and LA binder were added in a mass ratio of 8:1:1 to form a slurry, which was evenly coated on aluminum foil to obtain a positive electrode sheet. The negative electrode was a metal lithium sheet, and the electrolyte consisted of EC, DMC, and EMC containing 1.0M LiPF6 in a volume ratio of 1:1:1. The battery was assembled in an argon atmosphere glove box and put on the shelf for testing after 6 hours. The test voltage range was 2-4.8 V.

[0027] First, use a current density of 25 mA g –1 Then, the –1 The current density was cycled for 250 times to compare the discharge specific capacity, capacity retention rate, voltage, voltage retention rate, and voltage loss of the lithium-rich manganese-based positive electrode material (comparative example) and the anion-cation co-doped lithium-rich manganese-based positive electrode material (Examples 1-3). The results are as follows: Figure 2-7 As shown, the data are recorded in Table 1.

[0028] Table 1 It can be seen from Table 1 that the anion-cation co-doped lithium-rich manganese-based positive electrode material prepared in the present invention has good cycle performance and exhibits excellent capacity stability and voltage stability. The performance of Example 2 is the most outstanding. –1 After 200 cycles at the same current density, the capacity retention rate is as high as 100%, and the voltage retention rate is 92.9%.

[0029] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.

Claims

1. Anion-cation co-doped lithium-rich manganese-based positive electrode material, It is characterized in that The chemical formula of the positive electrode material is LiA 1-w [Li 1-x-2y Ni x Co y Mn 2-2x-y / 3 ]O 2-z B z , where 0.05<x≤0.25; 0.05≤y≤0.25; 0.7≤x+2y≤1; 0<z≤0.1; 0.9<w≤1; A is Na, B is F or S.

2. A method for preparing the anion-cation co-doped lithium-rich manganese-based positive electrode material as claimed in claim 1, It is characterized in that The steps include: 1) Ni-Co-Mn ternary precursor Ni x Co y Mn 2-2x-y / 3 (OH) a , where 0.05<x≤0.25, 0.05≤y≤0.25, 0.7≤x+2y≤1, 1.5≤a≤3, put into an aqueous solution of a compound containing elements A and B, stir to fully dissolve the sample, transfer to a polytetrafluoroethylene reactor for hydrothermal reaction; after the reaction, the sample is cooled and allowed to stand, centrifuged, washed and dried; 2) Grind the treated precursor and lithium carbonate in a mortar, mix thoroughly and pre-sinter, then heat and calcine, and grind thoroughly after cooling in the furnace to obtain anion-cation co-doped lithium-rich manganese-based positive electrode material.

3. The method for preparing the anion-cation co-doped lithium-rich manganese-based positive electrode material according to claim 2, It is characterized in that The compound containing elements A and B is Na 2 S.9H 2 O or NaF.

4. The method for preparing the anion-cation co-doped lithium-rich manganese-based positive electrode material according to claim 2, It is characterized in that In the step 1), the mass ratio of the nickel-cobalt-manganese ternary precursor to the compound containing elements A and B is 1:0.5-1.

5. The method for preparing the anion-cation co-doped lithium-rich manganese-based positive electrode material according to claim 2, It is characterized in that In the step 2), the mass ratio of the treated precursor to lithium carbonate is 1:0.66-1.

6. The method for preparing the anion-cation co-doped lithium-rich manganese-based positive electrode material according to claim 2, It is characterized in that In step 2), the pre-calcination heating rate is 2-10 ℃ / min –1 , calcined at 400-600℃ for 4-6 h; the heating rate of calcination is 5-15℃ / min –1 , calcined at 800-1000℃ for 10-20 h.

7. A lithium ion battery, It is characterized in that It comprises the anion-cation co-doped lithium-rich manganese-based positive electrode material as claimed in claim 1.

Citation Information

Cited By

  • Preparation method of Zr-doped modified lithium-rich manganese-based positive electrode material

    CN120271055A

  • Tungsten-doped high-nickel cobalt-free material and preparation method thereof

    CN120535030A