Resin-based hard carbon negative electrode material and preparation method and application thereof
Through the combination of amine or amino acid catalysts and zinc salt pore-forming agents, the pore structure of phenolic resin is optimized, and the performance and cost control problems of sodium ion battery negative electrode materials are solved, and the preparation of negative electrode materials with high capacity and high first-effect effects is achieved, which is suitable for commercial use. .
Patent Information
- Application Number
- CN202411147582.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-29
AI Technical Summary
The existing sodium ion battery negative electrode materials have problems such as low first-term efficiency, poor rate performance and poor cycle performance. In particular, the performance stability and cost control of hard carbon materials are difficult to achieve, and traditional acid and alkali catalysts are difficult to accurately control the pore structure of phenolic resins.
Using amines or amino acids as catalysts, combined with zinc salt pore-forming agents and ethylenediaminetetraacetic acid as stabilizers, optimize the pore structure and micropore characteristics of phenolic resins through low-temperature pre-carbonization and high-temperature carbonization processes to form high capacity and high-head Effective sodium ion battery negative electrode material.
The structural uniformity and performance stability of phenolic resin carbon are achieved, the preparation cost is reduced, the process flow is simplified, the electrochemical activity and controllability of the negative electrode material of sodium ion battery is improved, and it is suitable for large-scale production.
Smart Images

Figure CN119050350A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of carbon materials and new energy materials, and in particular relates to a resin-based hard carbon negative electrode material and a preparation method and application thereof. Background Art
[0002] Energy is the foundation of social development, so energy storage is extremely important. Among many batteries, sodium-ion batteries have the advantages of abundant resource reserves, low cost, and good safety performance, which are attracting the attention of scientific researchers and entrepreneurs. Among them, the design of positive and negative electrode materials plays a vital role. Unfortunately, despite breakthroughs in electrolyte and material design, graphite, as a negative electrode material for commercial lithium batteries, is difficult to store a large amount of Na ions. Therefore, if sodium-ion batteries want to achieve industrial breakthroughs, it is crucial to find a suitable and practical negative electrode material.
[0003] Among many negative electrode materials, hard carbon materials have the advantages of stable structure, low price, small volume deformation after sodium insertion, environmental friendliness and low redox potential, which are very suitable for commercialization. However, hard carbon negative electrodes are still constrained by bottlenecks such as low initial efficiency, poor rate performance and poor cycle performance. These performance indicators are the key to promoting the commercialization of sodium-ion batteries. Biomass materials are one of the earliest industrialized hard carbon precursors due to their rich raw materials and high capacity. However, there are regional and seasonal differences in raw materials, and performance stability is difficult to guarantee. Asphalt-based materials are widely available and low in cost, but the capacity of the product is difficult to increase. The hard carbon products obtained from resin precursors have good uniformity and high purity. And because the raw materials are controllable and the process is highly designed, the performance of the samples is very stable, but the disadvantage is that the cost is high. New technologies are urgently needed to prepare low-cost and high-performance resin hard carbon materials.
[0004] As a hard carbon precursor, phenolic resin has been widely studied due to its low cost, natural preparation, high carbon residue rate and excellent performance. How to precisely control the pore size, pore size distribution, pore type and other characteristics of phenolic resin carbon is the key to achieving high-performance hard carbon anode.
[0005] It is not easy to accurately control the polymerization reaction using traditional acid-base catalysts, and it is difficult to ensure the uniform structure of the phenolic resin. Summary of the invention
[0006] In view of the above technical problems, the purpose of the present invention is to prepare a resin-based hard carbon negative electrode material. By selecting amines as catalysts, phenolic resins with uniform pore structures can be synthesized in a controllable manner. Before polymerization, the pore former is evenly dispersed in the system, and the pore former reacts with C while carbonizing at low temperature to in-situ etch the carbon wall to produce micropores, thereby further optimizing the micropore specific surface area of phenolic resin carbon. Subsequently, during the high-temperature carbonization process, the pore structure of the hard carbon is regulated to prepare a negative electrode material for sodium ion batteries with high capacity, high initial efficiency and stable performance.
[0007] The technical solution of the present invention is as follows:
[0008] A resin-based hard carbon negative electrode material, characterized in that it comprises the following raw materials: a phenol monomer, an aldehyde monomer, a catalyst, a pore former, and a stabilizer;
[0009] The catalyst includes at least one of asparagine, ethylenediamine, dimethylamine, trimethylamine, 1,6-hexanediamine, diethylenetriamine, lysine, glutamic acid, aspartic acid and the like.
[0010] Preferably, the phenol monomer comprises at least one of phenol, resorcinol, catechol and phloroglucinol;
[0011] And / or, the aldehyde monomer includes at least one of formaldehyde, acetaldehyde and glyoxal.
[0012] Preferably, the molar ratio of phenol monomer to aldehyde monomer is 0.5 to 2:1;
[0013] and / or, the molar ratio of phenol monomer to catalyst is 10 to 20:1;
[0014] And / or, the molar ratio of the aldehyde monomer to water is 1:1-5.
[0015] The pore-forming agent is a zinc salt pore-forming agent, preferably at least one of zinc chloride, zinc nitrate and zinc acetate;
[0016] And / or, the stabilizer is ethylenediaminetetraacetic acid.
[0017] Preferably, the molar ratio of the aldehyde monomer to the pore-forming agent is 10 to 30:1;
[0018] And / or, the molar ratio of the pore-forming agent to ethylenediaminetetraacetic acid is 2 to 8:1.
[0019] The method for preparing the resin-based hard carbon negative electrode material is characterized by comprising the following steps:
[0020] (1) heating and melting or dissolving a phenol monomer in solution 1, and stirring the mixture with a catalyst to obtain a mixed solution A;
[0021] (2) dispersing the aldehyde monomer in solution 2, then adding a pore former and a stabilizer, and stirring evenly to obtain a mixed solution B;
[0022] (3) adding the mixed solution B prepared in step (2) to the mixed solution A obtained in step (1), keeping heating and stirring evenly, to obtain a mixed solution C;
[0023] (4) subjecting the mixed solution C prepared in step (3) to a polymerization reaction;
[0024] (5) After the reaction in step (4) is completed, the phenolic resin-based hard carbon is obtained by drying and then subjecting to low-temperature pre-carbonization and high-temperature carbonization.
[0025] Preferably, the solution 1 in step (1) is water;
[0026] and / or, the solution 2 in step (2) is water;
[0027] And / or, the polymerization reaction conditions of step (4) are: temperature 100-200° C., time 1-10 h.
[0028] Preferably, the low-temperature pre-carbonization in step (5) is carried out at a temperature of 500 to 1000° C. for a time of 1 to 4 hours; preferably, the carbonization atmosphere of the low-temperature carbonization is an inert gas;
[0029] And / or, the temperature of high-temperature carbonization is 1200-1800° C., and the time is 1-6 hours; preferably, the carbonization atmosphere of high-temperature carbonization is an inert gas.
[0030] Another object of the present invention is to protect the application of the above-mentioned phenolic resin-based hard carbon negative electrode material or the phenolic resin-based hard carbon negative electrode material prepared by the above-mentioned method in sodium ion batteries.
[0031] Using amines or amino acids as catalysts, polymerization can occur in a short time, shortening the cycle of polymerization. At the same time, in the process of polymerization, amines can also be used as N sources, and the doping of N elements can effectively improve the surface chemical properties of phenolic resin carbon. The present invention selects amines or amino acids as catalysts, has the advantages of preparing uniformly structured phenolic resins quickly and without residue, ensures the pore size and uniform distribution of phenolic resins, and reduces the irritation and toxicity of the reaction process. And avoids the problems of equipment requirements and environmental pollution caused by catalysts such as acids and alkalis, shortening the preparation cycle. In addition, Zn-type pore-forming agents are uniformly dispersed in phenolic resins for in-situ etching, and the pore structure is further optimized to prepare carbon with rich microporous properties. After carbonization, a closed pore structure is formed, which is applied to the negative electrode of sodium ion batteries with good performance.
[0032] Compared with the prior art, the advantages of the present invention are:
[0033] 1. Different from traditional acid-base catalysts, using amines or amino acids as catalysts can promote the polymerization reaction while making the polymerization reaction mild and uniform, which is conducive to the formation of uniform pores in the phenolic resin carbon and a more uniform microstructure. At the same time, during the polymerization reaction, amines or amino acids can also be used as N sources. The doping of N elements can effectively improve the chemical properties of phenolic resin carbon and provide more electrochemical active sites. In addition, this type of organic catalyst does not have to worry about the problem of ash residue.
[0034] 2. Use zinc salt pore former to optimize the microporous properties of phenolic resin carbon. Introduce Zn element in the process of molecular assembly. During the carbonization process, the pore structure is optimized by etching the carbon wall with ZnO at high temperature, that is, ZnO reacts with C to be reduced to Zn. The boiling point of Zn is 908℃ and it can be evaporated at high temperature. The etched carbon wall can form a pore structure, and the main pores formed are micropores below 2nm.
[0035] 3. Zinc salts are often unstable in resin systems and easily precipitate, resulting in uneven structures. By adding ethylenediaminetetraacetic acid as a stabilizer, zinc salts can be evenly embedded in the resin structure, which is beneficial to controlling the pore structure of hard carbon.
[0036] 4. Through the regulation of carbonization temperature, the pore size distribution and pore structure of phenolic resin carbon are further adjusted to form a large number of closed pores, and finally achieve excellent performance of high capacity and high first coulombic efficiency. The sample preparation process is simple, there is no strict requirement for equipment, the cost is low, and it can be prepared in large quantities. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 This is a process diagram for preparing the phenolic resin-based hard carbon negative electrode material of the present invention;
[0038] Figure 2 is an electron microscope scanning image of the phenolic resin-based negative electrode material prepared in Example 1 of the present invention;
[0039] Figure 3 The charge and discharge curve of the phenolic resin-based negative electrode material of Example 1 of the present invention as the negative electrode of a sodium ion battery at 0.1C. DETAILED DESCRIPTION
[0040] The present invention is further described in detail below in conjunction with specific embodiments, but the embodiments of the present invention are not limited thereto.
[0041] Example 1
[0042] A method for preparing a resin-based hard carbon negative electrode material comprises the following steps:
[0043] (1) 0.05 mol of phenol was heated to 60°C to melt into liquid form, and then mixed with 0.005 mol of 1,6-hexanediamine to obtain a mixed solution A.
[0044] (2) Take 0.2 mol of formaldehyde, add 1.0 mol of water, 0.01 mol of ethylenediaminetetraacetic acid and 0.02 mol of ZnCl2 in sequence, stir to dissolve, and stir evenly to obtain a mixed solution B.
[0045] (3) Add the mixed solution B prepared in step (2) to the mixed solution A obtained in step (1), keep heating, and stir evenly to obtain a mixed solution C.
[0046] (4) The mixed solution C prepared in step (3) was transferred to a reactor and treated at 150° C. for 6 h.
[0047] (5) After drying the sample prepared in step (4), heat it to 910°C at a heating rate of 5°C / min in an argon atmosphere and keep it at that temperature for 3 hours. After grinding the prepared sample, heat it to 700°C at a heating rate of 10°C / min in an argon atmosphere, and then heat it to 1400°C at a heating rate of 4°C / min and keep it at that temperature for 4 hours.
[0048] Example 2
[0049] A method for preparing a resin-based hard carbon negative electrode material comprises the following steps:
[0050] (1) 0.6 mol of resorcinol was dissolved in 1 mol of water at 60°C, and 0.03 mol of 1,6-hexanediamine was added and stirred evenly to prepare a mixed solution A.
[0051] (2) Take 0.3 mol of formaldehyde, add 0.3 mol of water, 0.0013 mol of ethylenediaminetetraacetic acid and 0.01 mol of Zn(NO3)2 in sequence, stir to dissolve, and stir evenly to obtain a mixed solution B.
[0052] (3) Add the mixed solution B prepared in step (2) to the mixed solution A obtained in step (1), keep heating, and stir evenly to obtain a mixed solution C.
[0053] (4) The mixed solution B prepared in step (3) was transferred to a reactor and treated at 120°C for 3 h.
[0054] (5) After drying the sample prepared in step (4), heat it to 930°C at a heating rate of 5°C / min in an argon atmosphere and keep it at that temperature for 2 hours. After grinding the prepared sample, heat it to 700°C at a heating rate of 10°C / min in an argon atmosphere, and then heat it to 1400°C at a heating rate of 4°C / min and keep it at that temperature for 4 hours.
[0055] Example 3
[0056] A method for preparing a resin-based hard carbon negative electrode material comprises the following steps:
[0057] (1) 0.3 mol of phenol was heated to 60°C to melt into liquid form, and then mixed with 0.03 g of 1,6-hexanediamine to obtain a mixed solution A.
[0058] (2) Take 0.3 mol of formaldehyde, add 0.6 mol of water, 0.01 mol of ethylenediaminetetraacetic acid and 0.03 mol of (CH3COO)2Zn in sequence, stir to dissolve, and stir evenly to obtain a mixed solution B.
[0059] (3) Add the mixed solution B prepared in step (2) to the mixed solution A obtained in step (1), keep heating, and stir evenly to obtain a mixed solution C.
[0060] (4) The mixed solution B prepared in step (3) was transferred to a reactor and treated at 150°C for 6 h.
[0061] (5) After drying the sample prepared in step (4), heat it to 950°C at a heating rate of 5°C / min in an argon atmosphere and keep it at that temperature for 2 hours. After grinding the prepared sample, heat it to 700°C at a heating rate of 10°C / min in an argon atmosphere, and then heat it to 1500°C at a heating rate of 4°C / min and keep it at that temperature for 4 hours.
[0062] Comparative Example 1
[0063] A method for preparing a resin-based hard carbon negative electrode material comprises the following steps:
[0064] (1) 0.05 mol of phenol is heated to 60°C to melt into a liquid state, and then mixed with 0.005 mol of sodium hydroxide to obtain a mixed solution A.
[0065] (2) 0.2 mol of formaldehyde is added to the mixed solution A obtained in step (1), and the mixture is heated and stirred to obtain a mixed solution B.
[0066] (3) The mixed solution B prepared in step (2) was transferred to a reactor and treated at 130°C for 4 h.
[0067] (4) After drying the sample prepared in step (3), heat it to 600°C at a heating rate of 5°C / min in an argon atmosphere and keep it at that temperature for 2 hours. After grinding the prepared sample, heat it to 700°C at a heating rate of 10°C / min in an argon atmosphere, and then heat it to 1500°C at a heating rate of 4°C / min and keep it at that temperature for 4 hours.
[0068] Comparative Example 2
[0069] A method for preparing a resin-based hard carbon negative electrode material comprises the following steps:
[0070] (1) Heat 0.05 mol of phenol to 60°C to melt it into a liquid state, and stir it evenly with 0.005 mol of hydrochloric acid to obtain a mixed solution A.
[0071] (2) 0.2 mol of formaldehyde is added to the mixed solution A obtained in step (1), and the mixture is heated and stirred to obtain a mixed solution B.
[0072] (3) The mixed solution B prepared in step (2) was transferred to a reactor and treated at 130°C for 4 h.
[0073] (4) After drying the sample prepared in step (3), heat it to 600°C at a heating rate of 5°C / min in an argon atmosphere and keep it at that temperature for 2 hours. After grinding the prepared sample, heat it to 700°C at a heating rate of 10°C / min in an argon atmosphere, and then heat it to 1500°C at a heating rate of 4°C / min and keep it at that temperature for 4 hours.
[0074] Comparative Example 3
[0075] A method for preparing a resin-based hard carbon negative electrode material comprises the following steps:
[0076] (1) 0.05 mol of phenol was heated to 60°C to melt into liquid form, and then mixed with 0.005 mol of 1,6-hexanediamine to obtain a mixed solution A.
[0077] (2) Take 0.2 mol of formaldehyde, add 1.0 mol of water, stir evenly, and prepare solution B.
[0078] (3) adding the solution B prepared in step (2) to the mixed solution A obtained in step (1), keeping heating and stirring evenly, to obtain a mixed solution C.
[0079] (4) The mixed solution C prepared in step (3) was transferred to a reactor and treated at 150° C. for 6 h.
[0080] (5) After drying the sample prepared in step (4), heat it to 910°C at a heating rate of 5°C / min in an argon atmosphere and keep it at that temperature for 3 hours. After grinding the prepared sample, heat it to 700°C at a heating rate of 10°C / min in an argon atmosphere, and then heat it to 1400°C at a heating rate of 4°C / min and keep it at that temperature for 4 hours.
[0081] Comparative Example 4
[0082] A method for preparing a resin-based hard carbon negative electrode material comprises the following steps:
[0083] (1) Dissolve 0.6 mol of resorcinol in 1 mol of water at 60°C, add 0.03 1,6-hexanediamine and stir evenly to prepare a mixed solution A.
[0084] (2) Take 0.3 mol of formaldehyde, add 0.3 mol of water, and stir evenly to prepare solution B.
[0085] (3) adding the solution B prepared in step (2) to the mixed solution A obtained in step (1), keeping heating and stirring evenly, to obtain a mixed solution C.
[0086] (4) The mixed solution B prepared in step (3) was transferred to a reactor and treated at 120°C for 3 h.
[0087] (5) After drying the sample prepared in step (4), heat it to 930°C at a heating rate of 5°C / min in an argon atmosphere and keep it at that temperature for 2 hours. After grinding the prepared sample, heat it to 700°C at a heating rate of 10°C / min in an argon atmosphere, and then heat it to 1400°C at a heating rate of 4°C / min and keep it at that temperature for 4 hours.
[0088] The hard carbon negative electrode materials prepared in Examples 1-3 and Comparative Examples 1-4 were subjected to performance tests, and the results are shown in Table 1.
[0089] Table 1: Test results of hard carbon negative electrode materials prepared in Examples 1-3 and Comparative Examples 1-4
[0090] Sodium storage reversible gram capacity (mAh / g) First coulombic efficiency (%) Example 1 363.5 90.2 Example 2 357.8 90.5 Example 3 352.4 90.4 Comparative Example 1 301.3 85.3 Comparative Example 2 310.5 85.1 Comparative Example 3 334.2 88.7 Comparative Example 4 328.1 88.5
[0091] The above contents are only basic descriptions of the concept of the present invention, and any equivalent changes made according to the technical solution of the present invention shall fall within the protection scope of the present invention.
Claims
1. A resin-based hard carbon negative electrode material, It is characterized in that The raw materials include: phenol monomer, aldehyde monomer, catalyst; The catalyst includes at least one of asparagine, ethylenediamine, dimethylamine, trimethylamine, 1,6-hexanediamine, diethylenetriamine, lysine, glutamic acid, aspartic acid and the like.
2. The resin-based hard carbon negative electrode material according to claim 1, It is characterized in that The phenol monomer includes at least one of phenol, resorcinol, catechol and phloroglucinol; And / or, the aldehyde monomer includes at least one of formaldehyde, acetaldehyde and glyoxal.
3. The resin-based hard carbon negative electrode material according to claim 1 or 2, It is characterized in that The molar ratio of phenol monomer to aldehyde monomer is 0.5 to 2:1; and / or, the molar ratio of phenol monomer to catalyst is 10 to 20:1; And / or, the molar ratio of the aldehyde monomer to water is 1:1-5.
4. The resin-based hard carbon negative electrode material according to claim 1 or 2, It is characterized in that The raw materials also include pore formers and stabilizers.
5. The resin-based hard carbon negative electrode material according to claim 4, It is characterized in that The pore-forming agent is a zinc salt pore-forming agent, preferably at least one of zinc chloride, zinc nitrate and zinc acetate; And / or, the stabilizer is ethylenediaminetetraacetic acid.
6. The resin-based hard carbon negative electrode material according to claim 4 or 5, It is characterized in that The molar ratio of the aldehyde monomer to the pore-forming agent is 10 to 30:1; And / or, the molar ratio of the pore-forming agent to ethylenediaminetetraacetic acid is 2 to 8:
1.
7. A method for preparing the resin-based hard carbon negative electrode material according to any one of claims 1 to 6, It is characterized in that The steps include: (1) heating and melting or dissolving a phenol monomer in solution 1, and stirring the mixture with a catalyst to obtain a mixed solution A; (2) dispersing the aldehyde monomer in solution 2, then adding a pore former and a stabilizer, and stirring evenly to obtain a mixed solution B; (3) adding the mixed solution B prepared in step (2) to the mixed solution A obtained in step (1), keeping heating and stirring evenly, to obtain a mixed solution C; (4) subjecting the mixed solution C prepared in step (3) to a polymerization reaction; (5) After the reaction in step (4) is completed, the phenolic resin-based hard carbon is obtained by drying and then subjecting to low-temperature pre-carbonization and high-temperature carbonization.
8. The preparation method according to claim 7, It is characterized in that The solution 1 in step (1) is water; and / or, the solution 2 in step (2) is water; And / or, the polymerization reaction conditions of step (4) are: temperature 100-200° C., time 1-10 h.
9. The preparation method according to claim 8, It is characterized in that The low-temperature pre-carbonization in step (5) is carried out at a temperature of 500 to 1000° C. for a time of 1 to 4 hours. Preferably, the carbonization atmosphere of the low-temperature carbonization is an inert gas. And / or, the temperature of high-temperature carbonization is 1200-1800° C., and the time is 1-6 hours; preferably, the carbonization atmosphere of high-temperature carbonization is an inert gas.
10. Use of the resin-based hard carbon negative electrode material according to any one of claims 1 to 6 or the resin-based hard carbon negative electrode material prepared by the method according to any one of claims 7 to 9 as a battery material, preferably, as a negative electrode material.
Citation Information
Cited By
Modified phenolic resin-based hard carbon material as well as preparation method and application thereof
CN119841303A
A modified phenolic resin-based hard carbon material and its preparation method and application
CN119841303B