Preparation method of modified ammonium polyphosphate flame-retardant PEO-based solid electrolyte membrane

Modified ammonium polyphosphate (TiO2@PA-APP) prepared by using chemical grafting method and microcapsule coating method in lithium-ion batteries, the flammable and low-temperature performance problems of liquid electrolytes in lithium-ion batteries are solved, and the problem of poor performance of liquid electrolytes in lithium-ion batteries is improved. The ionic conductivity and flame retardant properties of the electrolyte are achieved, and higher safety and reliability are achieved, and the production process is simplified.

CN119050463APending Publication Date: 2024-11-29KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411160870.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The liquid electrolytes used in traditional lithium-ion batteries have problems such as flammable, leak-prone and poor low-temperature performance, which limits the safety and reliability of lithium-ion batteries. The flammable components and low-temperature ion conductivity of existing polymer solid electrolytes It is difficult to widely use in lithium-ion batteries.

Method used

Modified ammonium polyphosphate (TiO2@PA-APP) was prepared by chemical grafting method and microcapsule coating method, and titanium oxide was introduced into the polymer solid electrolyte to form a composite material with good compatibility and improve the ions of the electrolyte. Conductivity and flame retardant properties, and simplify the process flow through DMF solvent and suitable reaction conditions.

Benefits of technology

It significantly improves the lithium-ion conductivity and flame retardant properties of the solid electrolyte membrane, enhances the thermal stability and electrochemical properties of the electrolyte, reduces production costs, and is suitable for large-scale industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050463A_ABST
    Figure CN119050463A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium ion battery solid electrolyte, in particular to a preparation method of a modified ammonium polyphosphate flame-retardant PEO-based solid electrolyte membrane, which comprises the following steps: S1, selecting ammonium polyphosphate, treating with a chemical grafting method and a microcapsule coating method, and drying in a vacuum environment to obtain modified ammonium polyphosphate (TiO2 (at) PA-APP) powder; s2, adding the powder in the S1 and PEO-based solid electrolyte powder into a DMF solvent, stirring at a constant temperature, and fully dissolving to obtain electrolyte slurry; s3, pouring the electrolyte slurry obtained in S2 into a polytetrafluoroethylene forming mold, and drying to obtain an electrolyte membrane; the PA-APP prepared by a chemical grafting method can also exert good flame retardant property under the condition that the addition amount of the flame retardant is very small, and the thermal stability of the electrolyte is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion battery solid electrolytes, and in particular to a method for preparing a modified ammonium polyphosphate flame-retardant PEO-based solid electrolyte membrane. Background Art

[0002] With the rapid development of portable electronic devices and electric vehicles, the demand for high energy density and high safety batteries is increasing. Lithium-ion batteries have become the mainstream choice due to their high energy density and long cycle life. However, the liquid electrolytes used in traditional lithium-ion batteries have problems such as flammability, leakage and poor low-temperature performance, which seriously affect the safety and reliability of the batteries.

[0003] Replacing liquid electrolytes and organic separators with solid electrolytes is a fundamental measure to solve the above problems. Among all solid electrolytes, polymer solid electrolytes have become a research hotspot due to their advantages such as low cost, good interface contact, excellent flexibility and film-forming properties. However, due to the inherent limitations of polymer solid electrolytes, such as the presence of flammable organic components and poor ionic conductivity at room temperature, it is difficult to be widely used in lithium-ion batteries. Therefore, modifying polymer solid electrolytes to improve their ionic conductivity and safety is of great significance to the development of all-solid-state lithium-ion batteries.

[0004] The existing Chinese patent document CN202011538865.5 discloses a silicone-modified phytate-coupled ammonium polyphosphate and a fire-retardant coating prepared therefrom. The epoxy silane coupling agent and the phytic acid metal salt are added to the ammonium polyphosphate in proportion and mixed evenly. The modification reaction is carried out at high temperature for a period of time, and the mixture is crushed to obtain a phytate-coupled ammonium polyphosphate with high phosphorus content and good fluidity. The fire-retardant coating prepared by mixing the phytate-coupled ammonium polyphosphate with other synergists has extended the stability and storage time of the coating. The fire resistance time measured under the fire resistance limit test can reach up to 120 minutes. The carbon layer after combustion is dense and continuous, has good bonding with the base plate, and does not fall off. The performance in all aspects is better than the fire-retardant coating made from the existing commercially available APP.

[0005] Compared with this technical solution, the modification conditions of ammonium polyphosphate in the patent are more stringent and require a high temperature environment. The corresponding application in practice will result in higher production costs. However, the modification conditions in this technical solution are very simple. It only requires adding the corresponding raw materials, controlling the reaction temperature at 90°C, and completing it under a nitrogen atmosphere. The process is simple, the preparation is convenient, and the cost of large-scale production is reduced.

[0006] In summary, exploring a solid electrolyte with high ionic conductivity, lithium ion migration ability and good flame retardancy is of great significance to the development of lithium-ion batteries. Summary of the invention

[0007] The purpose of the present invention is to provide a method for preparing a modified ammonium polyphosphate flame-retardant PEO-based solid electrolyte membrane. The modified ammonium polyphosphate (TiO2@PA-APP) in the present invention is a new type of environmentally friendly phosphorus-nitrogen flame retardant; PA-APP prepared by chemical grafting can also exert good flame retardant properties when the amount of flame retardant added is very small, thereby improving the thermal stability of the electrolyte. In addition, a layer of TiO2 is further coated on the outside of PA-APP by a microcapsule coating method, which can not only enhance the compatibility of the flame retardant material with the polymer solid electrolyte, but also improve the ionic conductivity and lithium ion migration ability of the electrolyte.

[0008] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:

[0009] A method for preparing a modified ammonium polyphosphate flame-retardant PEO-based solid electrolyte membrane comprises the following steps:

[0010] S1: Select ammonium polyphosphate, treat it by chemical grafting and microencapsulation, and dry it in a vacuum environment to obtain modified ammonium polyphosphate (TiO2@PA-APP) powder, such as Figure 1 As shown;

[0011] S2: Add the powder in S1 and the PEO-based solid electrolyte powder into DMF solvent, stir at a constant temperature, and obtain electrolyte slurry after fully dissolving;

[0012] S3: pouring the electrolyte slurry obtained in S2 into a polytetrafluoroethylene forming mold, and obtaining an electrolyte membrane after drying;

[0013] Furthermore, the chemical grafting method in step S1 includes the following sub-steps:

[0014] S1.1.1: Add 70 mL of anhydrous ethanol and 4 mL of deionized water into a three-necked flask and stir for 30 min to obtain a uniform mixed solution;

[0015] S1.1.2: Add 4.3 g of piperazine (PA) to the mixed solution obtained in step S1.1.1 and stir until completely dissolved;

[0016] S1.1.3: Add 10 g of ammonium polyphosphate (APP) to the PA mixture obtained in step S1.1.2, and continue stirring until the pH value of the solution is between 8 and 9;

[0017] S1.1.4: After the reaction is completed, the obtained substance is cooled to room temperature, washed and filtered with anhydrous ethanol, and then dried in a vacuum drying oven at 90°C to constant weight to obtain piperazine-modified ammonium polyphosphate (PA-APP) solid.

[0018] Furthermore, in steps S1-S3, the temperature of all reactions was set at 90°C and completed under a nitrogen atmosphere.

[0019] Furthermore, the microcapsule coating method in step S1 includes the following sub-steps:

[0020] S1.2.1: Dissolve 10 g of the PA-APP solid obtained in step S1.1.4 in anhydrous ethanol and stir at 90°C for 10 min to obtain a mixed solution;

[0021] S1.2.2: Add a mixed solution containing 3.5 g of tetrabutyl titanate and 0.74 g of aqueous ammonia to the mixed solution obtained in step S1.2.1, and stir for 5 h;

[0022] S1.2.3: Cool the mixed solution obtained in step S1.2.2 to room temperature, then wash with anhydrous ethanol and filter.

[0023] Furthermore, the vacuum drying temperature in step S1 is 90° C. and the drying time is 24 h;

[0024] Furthermore, in step S2, the mass of the TiO2@PA-APP powder is 1%-4% of the mass of the PEO-based solid electrolyte powder, and the mass ratio of the DFM solvent to the PEO-based solid electrolyte powder is 12:1.

[0025] Furthermore, in step S2, the PEO-based solid electrolyte powder is a mixture of PEO, LiTFSI, PVDF and Al2O3 in a mass ratio of 12:4:3:1.

[0026] Furthermore, the dissolving method in step S2 is stirring at a stirring speed of 100-200 r / min at a constant temperature of 60° C. for 24 hours.

[0027] Furthermore, the drying method in step S3 is to cure in a constant temperature oven at 40°C for 12 hours, and then dry in a vacuum drying oven at a constant temperature of 50°C-60°C for 24 hours.

[0028] Beneficial effects of the present invention:

[0029] The present invention significantly improves the lithium ion conductivity of the solid electrolyte membrane. This is achieved by introducing titanium oxide (TiO2) into ammonium polyphosphate (PA-APP). TiO2 itself is an ion conductor, and its microstructure provides a migration channel for lithium ions, which can effectively promote the movement of lithium ions. In step S1, TiO2 is coated on the outer surface of PA-APP by a microencapsulation method to form a composite material with good compatibility. The Lewis acid effect of TiO2 can make TFSI -The anions are anchored on the surface of TiO2@PA-APP particles, which is beneficial to the dissociation of LiTFSI and releases more Li + transport, improving the ionic conductivity of solid electrolytes and Li + The TiO2@PA-APP proposed in the present invention can be considered as a flame retardant filler that can improve the electrochemical properties of the electrolyte.

[0030] The present invention significantly improves the flame retardant properties of the solid electrolyte membrane. As an excellent flame retardant, ammonium polyphosphate can release phosphoric acid substances during thermal decomposition to form a protective carbonized layer to isolate flames from combustibles. Through the comprehensive application of chemical grafting and microencapsulation coating, the prepared modified ammonium polyphosphate (TiO2@PA-APP) has excellent flame retardant properties. The TiO2 layer coated on the outside of PA-APP not only improves the compatibility of flame retardant materials and polymer electrolytes, allowing the flame retardant materials to be evenly distributed in the electrolyte, but also improves the electrochemical properties of the solid electrolyte.

[0031] The preparation method of the present invention significantly improves the thermal stability of the membrane. In step S1, a vacuum drying treatment at 90°C is used to remove moisture and volatile components in the material, which is crucial to improving the thermal stability of the membrane. The thermal weight loss rate of the material at high temperature is reduced, ensuring its structural integrity in a high temperature environment. In addition, the introduction of TiO2@PA-APP further improves the thermal stability of the membrane. During the combustion of the electrolyte membrane, the TiO2 layer on the surface of TiO2@PA-APP is ruptured by heat, releasing the internal PA-APP. PA-APP decomposes to generate PNC structure and polyphosphoric acid, while releasing NH3 and H2O. The C=C and PNC structures thus formed help to form a stable carbon layer on the surface of the PEO matrix, delaying the exchange of combustible substances and heat conduction, thereby slowing down the decomposition rate of the internal matrix. Therefore, under extreme operating conditions, the thermal stability of the electrolyte membrane helps to enhance the overall safety and reliability of the battery and ensure the stable performance of the battery in long-term use.

[0032] Finally, the preparation method of the present invention provides convenient conditions for industrial production. By optimizing the reaction steps, such as using DMF as a solvent in step S2, it is possible to achieve sufficient dissolution of PEO and the composite material in a relatively short time, ensuring the uniformity and molding quality of the film. In addition, the required reaction temperature and vacuum environment conditions are moderate, and compared with the preparation method of traditional solid electrolytes, it has lower energy consumption and a more simplified process flow, which is convenient for large-scale production. This production method not only reduces production costs, but also helps to realize the mass application of high-performance electrolyte materials and promote the widespread application and marketization of lithium-ion battery technology.

[0033] In summary, the preparation method of the modified ammonium polyphosphate flame-retardant PEO-based solid electrolyte membrane of the present invention not only significantly improves the performance of the electrolyte membrane in terms of lithium ion conductivity, flame retardancy, thermal stability and industrial production, but its internal mechanism also fully reflects the cross-application of materials science and engineering, providing an effective solution for the development of lithium-ion batteries.

[0034] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0036] Figure 1 This is a schematic diagram of the preparation of TiO2@PA-APP flame retardant;

[0037] Figure 2 It is a test data diagram of ionic conductivity of the modified ammonium polyphosphate flame-retardant PEO-based solid electrolyte membrane prepared in Examples 1-4 and Comparative Example 1;

[0038] Figure 3 TG test graph of the modified ammonium polyphosphate flame-retardant PEO-based solid electrolyte membrane prepared in Examples 1-2 and Comparative Example 1;

[0039] Figure 4 This is a graph of heat release rate of the modified ammonium polyphosphate flame-retardant PEO-based solid electrolyte membrane prepared in Example 2 and Comparative Example 1. DETAILED DESCRIPTION

[0040] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] Example 1

[0042] A method for preparing a modified ammonium polyphosphate flame-retardant PEO-based solid electrolyte membrane as described in this embodiment comprises the following steps:

[0043] S1: 70 mL of anhydrous ethanol and 4 mL of deionized water were added to a three-necked flask, respectively, and stirred for 30 min to obtain a uniform mixed solution. 4.3 g of piperazine (PA) was added to the mixed solution and stirred until completely dissolved. Then, 10 g of ammonium polyphosphate (APP) was added to the PA mixed solution and stirred continuously until the pH value of the solution was between 8 and 9. The temperature of the entire reaction was controlled at 90°C and carried out under a nitrogen atmosphere. After the reaction was completed, the reaction product was cooled to room temperature, washed and filtered with anhydrous ethanol, and then dried in a vacuum drying oven at 90°C to constant weight to obtain piperazine-modified ammonium polyphosphate (PA-APP) solid.

[0044] S2: Take 10g of the PA-APP solid obtained by the above reaction and dissolve it in anhydrous ethanol, stir it at 90°C for 10 minutes to obtain a mixed solution, then add a mixed solution containing 3.5g of tetrabutyl titanate and 0.74g of ammonia water, stir for 5 hours, then cool the mixed solution to room temperature, wash and filter it with anhydrous ethanol, and dry it in a vacuum drying oven at 90°C for 24 hours to obtain TiO2@PA-APP powder.

[0045] S3: Weigh 0.02 g TiO2@PA-APP powder, 1.2 g PEO, 0.4 g LiTFSI, 0.3 g PVDF, and 0.1 g Al2O3 into a serum bottle.

[0046] S4: Take 27 ml of DMF solvent and add it into a serum bottle. Stir it at a constant temperature of 60° C. and a speed of 150 r / min for 24 h to obtain a PEO-based electrolyte slurry after it is fully dissolved.

[0047] S5: pour the PEO-based electrolyte slurry obtained in step S4 into a polytetrafluoroethylene molding mold, place it in a constant temperature oven at 40° C. for curing for 12 hours, and then dry it in a vacuum drying oven at a constant temperature of 60° C. for 24 hours to obtain an electrolyte membrane.

[0048] Example 2

[0049] A method for preparing a modified ammonium polyphosphate flame-retardant PEO-based solid electrolyte membrane as described in this embodiment comprises the following steps:

[0050] S1: 70 mL of anhydrous ethanol and 4 mL of deionized water were added to a three-necked flask, respectively, and stirred for 30 min to obtain a uniform mixed solution. 4.3 g of piperazine (PA) was added to the mixed solution and stirred until completely dissolved. Then, 10 g of ammonium polyphosphate (APP) was added to the PA mixed solution and stirred continuously until the pH value of the solution was between 8 and 9. The temperature of the entire reaction was controlled at 90°C and carried out under a nitrogen atmosphere. After the reaction was completed, the reaction product was cooled to room temperature, washed and filtered with anhydrous ethanol, and then dried in a vacuum drying oven at 90°C to constant weight to obtain piperazine-modified ammonium polyphosphate (PA-APP) solid.

[0051] S2: Take 10g of the PA-APP solid obtained by the above reaction and dissolve it in anhydrous ethanol, stir it at 90°C for 10 minutes to obtain a mixed solution, then add a mixed solution containing 3.5g of tetrabutyl titanate and 0.74g of ammonia water, stir for 5 hours, then cool the mixed solution to room temperature, wash and filter it with anhydrous ethanol, and dry it in a vacuum drying oven at 90°C for 24 hours to obtain TiO2@PA-APP powder.

[0052] S3: Weigh 0.04 g TiO2@PA-APP powder, 1.2 g PEO, 0.4 g LiTFSI, 0.3 g PVDF, and 0.1 g Al2O3 into a serum bottle.

[0053] S4: Take 27 ml of DMF solvent and add it into a serum bottle. Stir it at a constant temperature of 60° C. and a speed of 150 r / min for 24 h to obtain a PEO-based electrolyte slurry after it is fully dissolved.

[0054] S5: pour the PEO-based electrolyte slurry obtained in step S4 into a polytetrafluoroethylene molding mold, place it in a 40°C oven for curing for 12 hours, and then dry it in a vacuum drying oven at a constant temperature of 60°C for 24 hours to obtain an electrolyte membrane.

[0055] Example 3

[0056] A method for preparing a modified ammonium polyphosphate flame-retardant PEO-based solid electrolyte membrane as described in this embodiment comprises the following steps:

[0057] S1: 70 mL of anhydrous ethanol and 4 mL of deionized water were added to a three-necked flask, respectively, and stirred for 30 min to obtain a uniform mixed solution. 4.3 g of piperazine (PA) was added to the mixed solution and stirred until completely dissolved. Then, 10 g of ammonium polyphosphate (APP) was added to the PA mixed solution and stirred continuously until the pH value of the solution was between 8 and 9. The temperature of the entire reaction was controlled at 90°C and carried out under a nitrogen atmosphere. After the reaction was completed, the reaction product was cooled to room temperature, washed and filtered with anhydrous ethanol, and then dried in a vacuum drying oven at 90°C to constant weight to obtain piperazine-modified ammonium polyphosphate (PA-APP) solid.

[0058] S2: Take 10g of the PA-APP solid obtained by the above reaction and dissolve it in anhydrous ethanol, stir it at 90°C for 10 minutes to obtain a mixed solution, then add a mixed solution containing 3.5g of tetrabutyl titanate and 0.74g of ammonia water, stir for 5 hours, then cool the mixed solution to room temperature, wash and filter it with anhydrous ethanol, and dry it in a vacuum drying oven at 90°C for 24 hours to obtain TiO2@PA-APP powder.

[0059] S3: Weigh 0.06 g TiO2@PA-APP powder, 1.2 g PEO, 0.4 g LiTFSI, 0.3 g PVDF, and 0.1 g Al2O3 into a serum bottle.

[0060] S4: Take 27 ml of DMF solvent and add it into a serum bottle. Stir it at a constant temperature of 60° C. and a speed of 150 r / min for 24 h to obtain a PEO-based electrolyte slurry after it is fully dissolved.

[0061] S5: pour the PEO-based electrolyte slurry obtained in step S4 into a polytetrafluoroethylene molding mold, place it in a 40°C oven for curing for 12 hours, and then dry it in a vacuum drying oven at a constant temperature of 60°C for 24 hours to obtain an electrolyte membrane.

[0062] Example 4

[0063] A method for preparing a modified ammonium polyphosphate flame-retardant PEO-based solid electrolyte membrane as described in this embodiment comprises the following steps:

[0064] S1: 70 mL of anhydrous ethanol and 4 mL of deionized water were added to a three-necked flask, respectively, and stirred for 30 min to obtain a uniform mixed solution. 4.3 g of piperazine (PA) was added to the mixed solution and stirred until completely dissolved. Then, 10 g of ammonium polyphosphate (APP) was added to the PA mixed solution and stirred continuously until the pH value of the solution was between 8 and 9. The temperature of the entire reaction was controlled at 90°C and carried out under a nitrogen atmosphere. After the reaction was completed, the reaction product was cooled to room temperature, washed and filtered with anhydrous ethanol, and then dried in a vacuum drying oven at 90°C to constant weight to obtain piperazine-modified ammonium polyphosphate (PA-APP) solid.

[0065] S2: Take 10g of the PA-APP solid obtained by the above reaction and dissolve it in anhydrous ethanol, stir it at 90°C for 10 minutes to obtain a mixed solution, then add a mixed solution containing 3.5g of tetrabutyl titanate and 0.74g of ammonia water, stir for 5 hours, then cool the mixed solution to room temperature, wash and filter it with anhydrous ethanol, and dry it in a vacuum drying oven at 90°C for 24 hours to obtain TiO2@PA-APP powder.

[0066] S3: Weigh 0.08 g TiO2@PA-APP powder, 1.2 g PEO, 0.4 g LiTFSI, 0.3 g PVDF, and 0.1 g Al2O3 into a serum bottle.

[0067] S4: Take 27 ml of DMF solvent and add it into a serum bottle. Stir it at a constant temperature of 60° C. and a speed of 150 r / min for 24 h to obtain a PEO-based electrolyte slurry after it is fully dissolved.

[0068] S5: pour the PEO-based electrolyte slurry obtained in step S4 into a polytetrafluoroethylene molding mold, place it in a 40°C oven for curing for 12 hours, and then dry it in a vacuum drying oven at a constant temperature of 60°C for 24 hours to obtain an electrolyte membrane.

[0069] Example 5

[0070] Comparative Example 1

[0071] A method for preparing a modified ammonium polyphosphate flame-retardant PEO-based solid electrolyte membrane as described in this embodiment comprises the following steps:

[0072] S1: Weigh 1.2 g PEO, 0.4 g LiTFSI, 0.3 g PVDF, and 0.1 g Al2O3 into a serum bottle for later use.

[0073] S2: Take 27 ml of DMF solvent and add it into a serum bottle. Stir it at a constant temperature of 60°C and a speed of 150 r / min for 24 hours to obtain a PEO-based electrolyte slurry after it is fully dissolved.

[0074] S3: pour the PEO-based electrolyte slurry obtained in step S2 into a polytetrafluoroethylene molding mold, place it in a 40°C oven for curing for 12 hours, and then dry it in a vacuum drying oven at a constant temperature of 60°C for 24 hours to obtain an electrolyte membrane.

[0075] Example 6

[0076] Performance Testing

[0077] Ionic conductivity test

[0078] The modified ammonium polyphosphate flame-retardant PEO-based electrolyte membranes prepared in Examples 1-4 and Comparative Example 1 were sandwiched between two stainless steel sheets and placed in a 60°C constant temperature oven to test the ionic conductivity. The test frequency range was 10 6 Hz-10 -1 Hz, see Table 1 and Table 2 for specific test results. Figure 2 .

[0079] Table 1 Battery performance corresponding to Examples 1 to 4 and Comparative Example 1

[0080] project <![CDATA[Ionic conductivity (S cm -1 )]]> Comparative Example 1 <![CDATA[9.12×10 -5 ]]> Example 1 <![CDATA[1.2×10 -4 ]]> Example 2 <![CDATA[1.5×10 -4 ]]> Example 3 <![CDATA[1.17×10 -4 ]]> Example 4 <![CDATA[1.01×10 -4 ]]>

[0081] It can be seen from Table 1 that the ionic conductivity of Examples 1-4 is higher than that of Comparative Example 1, and the ionic conductivity shows a trend of first increasing and then decreasing with the addition of TiO2@PA-APP flame retardant. Among them, the ionic conductivity of Example 2 is the highest. This shows that adding different amounts of TiO2@PA-APP flame retardant to PEO-based solid electrolytes can improve the ionic conductivity of solid electrolytes, but there is an optimal addition amount.

[0082] Flame retardant performance test

[0083] Thermogravimetric tests were performed on Examples 1-2 and Comparative Example 1.

[0084] 5-10 mg of the samples of Examples 1-2 and Comparative Example 1 were weighed and placed in a crucible. -1 The temperature was raised from room temperature to 800°C at a heating rate, and the mass change during the heating process was measured. Figure 3 .

[0085] pass Figure 3 It is known that the maximum carbon residue in Example 2 is 17.9%, and the quality remains stable at 400°C. The carbon residue of the PEO-based solid electrolyte membrane under the three conditions is in the following order from largest to smallest: Example 2> Example 1> Comparative Example 1. This shows that the addition of TiO2@PA-APP flame retardant improves the flame retardancy of the electrolyte membrane to a certain extent, and the improvement effect increases with the increase in the amount added.

[0086] Micro-cone measurement test was performed on Example 2 and Comparative Example 1.

[0087] Example 2 and comparative example 1 were cut into a size of 100 mm × 100 mm × 25 mm and subjected to micro-cone measurement. The test procedure was 1 ° C min -1 The rate of heating is from 40℃ to 800℃. For specific results, see Figure 4 .

[0088] The heat release rate of Comparative Example 1 reaches 919 W g-1, while the heat release rate of Example 2 is only 267 W g-1.

[0089] This shows that the addition of TiO2@PA-APP flame retardant significantly reduces the heat release rate of the electrolyte membrane, improves the thermal stability of the PEO-based solid electrolyte membrane, and improves the flame retardancy of the PEO-based solid electrolyte membrane to a certain extent.

[0090] Existing patent documents disclose the application of modified ammonium polyphosphate PA-APP in flame retardants. At the same time, titanium dioxide is added to the flame retardant. Its internal mechanism is: an appropriate amount of titanium dioxide will decompose APP to produce acidic substances and react to form titanium pyrophosphate, which is enriched on the surface of the substrate and plays a good barrier role.

[0091] The flame retardant mechanism of this technical solution is as follows: the modified ammonium polyphosphate flame retardant is added to the PEO-based electrolyte. When the electrolyte is heated, the titanium dioxide layer on the surface breaks and releases PA-APP. PA-APP decomposes to form a PNC structure and polyphosphoric acid, while releasing NH3 and H2O. The C=C and PNC structures thus formed help to form a stable carbon layer on the surface of the PEO matrix, delaying the exchange of combustible substances and heat conduction, thereby slowing down the decomposition rate of the internal matrix, thereby playing a flame retardant role and improving the thermal stability of the material. The TiO2 layer on the surface of PA-APP mainly plays a role in improving the compatibility of PA-APP with the polymer matrix and the electrochemical performance of the solid electrolyte. The reasons for the improvement in electrochemical performance are mainly from two aspects: (1) The incorporation of TiO2@PA-APP as a filler into the PEO-based polymer solid electrolyte membrane effectively inhibits the crystallization behavior of the polymer in the PEO matrix, thereby increasing the amorphous region, which is conducive to the transfer of Li through the movement of the polymer chain segments. + (2) Due to the Lewis acid effect of TiO2, TFSI - The anions are anchored on the surface of TiO2@PA-APP particles, which is beneficial to the dissociation of LiTFSI and releases more Li + transport, thereby improving ionic conductivity and Li +Transfer. TiO2@PA-APP added to the polymer electrolyte not only improves the flame retardancy and thermal stability of the PEO-based electrolyte to a certain extent, but also improves the electrochemical performance of the PEO-based electrolyte. Although the fire retardant coatings in the existing patent documents have excellent flame retardant properties, it is unknown whether they can improve the electrochemical performance of PEO-based polymer electrolytes.

[0092] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing a modified ammonium polyphosphate flame-retardant PEO-based solid electrolyte membrane, It is characterized in that The following steps are involved: S1: Select ammonium polyphosphate, treat it by chemical grafting method and microencapsulation method, and dry it in a vacuum environment to obtain modified ammonium polyphosphate powder; S2: Add the powder in S1 and the PEO-based solid electrolyte powder into DMF solvent, stir at a constant temperature, and obtain electrolyte slurry after fully dissolving; S3: pouring the electrolyte slurry obtained in S2 into a polytetrafluoroethylene molding mold, and obtaining an electrolyte membrane after drying.

2. The method for preparing the modified ammonium polyphosphate flame-retardant PEO-based solid electrolyte membrane according to claim 1, Features: The chemical grafting method in step S1 includes the following sub-steps: S1.1.1: Add 70 mL of anhydrous ethanol and 4 mL of deionized water into a three-necked flask and stir for 30 min to obtain a uniform mixed solution; S1.1.2: Add 4.3 g of piperazine to the mixed solution obtained in step S1.1.1 and stir until completely dissolved; S1.1.3: Add 10 g of ammonium polyphosphate to the PA mixture obtained in step S1.1.2, and continue stirring until the pH value of the solution is between 8 and 9; S1.1.4: After the reaction is completed, the obtained substance is cooled to room temperature, washed and filtered with anhydrous ethanol, and then dried in a vacuum drying oven at 90°C to constant weight to obtain piperazine-modified ammonium polyphosphate solid.

3. The method for preparing the modified ammonium polyphosphate flame-retardant PEO-based solid electrolyte membrane according to claim 1, Features: The microcapsule coating method in step S1 includes the following sub-steps: S1.2.1: Dissolve 10 g of the PA-APP solid obtained in step S1.1.4 in anhydrous ethanol and stir at 90°C for 10 min to obtain a mixed solution; S1.2.2: Add a mixed solution containing 3.5 g of tetrabutyl titanate and 0.74 g of aqueous ammonia to the mixed solution obtained in step S1.2.1, and stir for 5 h; S1.2.3: Cool the mixed solution obtained in step S1.2.2 to room temperature, then wash with anhydrous ethanol and filter.

4. The method for preparing the modified ammonium polyphosphate flame-retardant PEO-based solid electrolyte membrane according to claim 1, Features: The vacuum drying temperature in step S1 is 90° C. and the drying time is 24 hours.

5. The method for preparing the modified ammonium polyphosphate flame-retardant PEO-based solid electrolyte membrane according to claim 1, Features: In step S2, TiO 2 The mass of @PA-APP powder is 1%-4% of the mass of PEO-based solid electrolyte powder, and the mass ratio of DFM solvent to PEO-based solid electrolyte powder is 12:

1.

6. The method for preparing the modified ammonium polyphosphate flame-retardant PEO-based solid electrolyte membrane according to claim 1, Features: In step S2, the PEO-based solid electrolyte powder is composed of PEO, LiTFSI, PVDF and Al in a mass ratio of 12:4:3:

1. 2 O 3 Mixed.

7. The method for preparing the modified ammonium polyphosphate flame-retardant PEO-based solid electrolyte membrane according to claim 1, Features: The dissolving method in step S2 is to stir at a stirring speed of 100-200 r / min at a constant temperature of 60° C. for 24 hours.

8. The method for preparing the modified ammonium polyphosphate flame-retardant PEO-based solid electrolyte membrane according to claim 1, Features: The drying method in step S3 is to cure in a constant temperature oven at 40°C for 12 hours, and then dry in a vacuum drying oven at a constant temperature of 50°C-60°C for 24 hours.

Citation Information

Cited By

  • Flame-retardant microcapsule as well as preparation method and application thereof

    CN121288237A