Electrolyte and battery
By using low viscosity and high dielectric constant organic solvents and appropriate lithium salt concentrations in lithium-ion battery electrolytes, a stable SEI film is formed, which solves the problem of poor fast charging performance of lithium-ion batteries and achieves higher ionic conductivity and cycle stability.
Patent Information
- Application Number
- CN202411281579.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-29
AI Technical Summary
During the fast charging process, existing lithium-ion batteries have problems such as slow ion migration speed, high lithium-ion desolvation activation energy, and unstable SEI membranes, which affect fast charging performance.
By using organic solvents with viscosity less than 2.5 cp and dielectric constant greater than 30 in the electrolyte, such as acetonitrile and fluorovinyl carbonate, the lithium salt concentration is controlled between 0.1 and 4.0 mol/L to form a stable SEI film and improve lithium ions rapid decomposition and conduction.
It significantly improves the fast charging performance and cycle stability of lithium-ion batteries, reduces the irreversible loss of lithium ions, extends the cycle life of the battery, and maintains a high capacity under large-scale charging and discharging.
Smart Images

Figure CN119050471A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to an electrolyte and a battery. Background Art
[0002] Lithium-ion batteries (LIBs) with fast charging capabilities may be able to overcome the "range anxiety" problem and promote the wider application of electric vehicles. Electrolyte is a key material for lithium-ion batteries. By regulating the composition of the electrolyte, we can improve ionic conductivity, optimize the composition and structure of the solid electrolyte interface (SEI membrane), and reduce Li + The desolvation activation energy can be increased and the migration speed through SEI can be improved, thereby improving the fast charging performance of lithium-ion batteries. Summary of the invention
[0003] Embodiments of the present invention provide an electrolyte and a battery, which can improve the fast charging performance of a lithium-ion battery.
[0004] In a first aspect, an embodiment of the present invention provides an electrolyte, comprising a lithium salt and an organic solvent, wherein the viscosity η of the organic solvent is less than 2.5 cp and / or the dielectric constant ε of the organic solvent is greater than 30
[0005] In one embodiment, the viscosity η of the organic solvent is less than 2.3 cp and / or the dielectric constant ε of the organic solvent is greater than 35.
[0006] In one embodiment, the electrolyte consists of lithium salt and an organic solvent.
[0007] In one embodiment, the concentration of the lithium salt in the electrolyte is 0.1-4.0 mol / L.
[0008] In one embodiment, the organic solvent includes one or more of linear carbonates and their substituents, propylene carbonate and their substituents, ethylene carbonate and their substituents, linear carboxylates and their substituents, nitriles and their substituents, and sulfites and their substituents.
[0009] In one embodiment, the organic solvent includes at least one of ethylene carbonate and its substituents, and at least one of nitriles and their substituents.
[0010] In one embodiment, the organic solvent includes acetonitrile and fluoroethylene carbonate.
[0011] In one embodiment, the mass ratio of the acetonitrile to the fluoroethylene carbonate is (0.1-5):(5-10).
[0012] In one embodiment, the mass ratio of the acetonitrile to the fluoroethylene carbonate is 3:7.
[0013] In one embodiment, the lithium salt includes one or more of an inorganic lithium salt and an organic lithium salt, the inorganic lithium salt includes one or more of lithium perchlorate, lithium tetrafluoroborate, lithium hexafluoroarsenate and lithium hexafluorophosphate, and the organic lithium salt includes one or more of lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium bis(difluorosulfonylimide) and lithium bis(trifluoromethylsulfonylimide).
[0014] In a second aspect, an embodiment of the present invention provides a battery, comprising the above-mentioned electrolyte.
[0015] Beneficial effects of the embodiments of the present invention:
[0016] In an embodiment of the present invention, by controlling the viscosity of the organic solvent, the wetting effect of the electrolyte can be improved, thereby improving the fast charging performance of the electrolyte; by controlling the dielectric constant of the organic solvent, the lithium salt can be fully dissolved and quickly and fully decomposed into lithium ions and anions, thereby quickly providing sufficient lithium ions, thereby improving the fast charging performance of the electrolyte; at the same time, controlling the viscosity and dielectric constant of the organic solvent can more effectively improve the fast charging performance of the electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0018] Figure 1 It is a line graph of ionic conductivity of different electrolyte systems provided in the embodiments and comparative examples of the present invention in the temperature range of -30 to 60°C;
[0019] Figure 2 It is a structural schematic diagram of a three-electrode cylindrical capacitor test box used for dielectric constant testing in the present invention. DETAILED DESCRIPTION
[0020] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention. In the present invention, unless otherwise specified, the directional words used, such as "upper" and "lower", generally refer to the upper and lower parts of the device in actual use or working state, specifically the drawing direction in the drawings; while "inside" and "outside" refer to the outline of the device.
[0021] The technical solution of this application is as follows:
[0022] In a first aspect, an embodiment of the present application provides an electrolyte comprising a lithium salt and an organic solvent, wherein the viscosity η of the organic solvent is less than 2.5 cp and / or the dielectric constant ε of the organic solvent is greater than 30.
[0023] In the present application, by controlling the viscosity of the organic solvent, the wetting effect of the electrolyte can be improved, thereby improving the fast charging performance of the electrolyte; by controlling the dielectric constant of the organic solvent, the lithium salt can be fully dissolved and quickly and fully decomposed into lithium ions and anions, thereby quickly providing sufficient lithium ions, thereby improving the fast charging performance of the electrolyte; at the same time, controlling the viscosity and dielectric constant of the organic solvent can more effectively improve the fast charging performance of the electrolyte.
[0024] In the present application, the organic solvent may be a mixture of several solvents, and the viscosity and dielectric constant of the organic solvent refer to the viscosity and dielectric constant of the mixture of several solvents. The viscosity of the organic solvent η<2.5cp means that the viscosity of the organic solvent is less than 2.5cp at 25°C.
[0025] In one embodiment, the viscosity η of the organic solvent is less than 2.3 cp and / or the dielectric constant ε of the organic solvent is greater than 35. The viscosity η of the organic solvent is less than 2.3 cp, which means that the viscosity of the organic solvent is less than 2.3 cp at 25°C.
[0026] In some embodiments, the concentration of the lithium salt in the electrolyte is 0.1-4.0 mol / L, for example, 1.0 mol / L, 1.5 mol / L, 2.0 mol / L, 2.5 mol / L, 3.0 mol / L, 3.5 mol / L, 4.0 mol / L, etc. Within the range, the lithium salt concentration is moderate, sufficient lithium ions can be provided, and the viscosity is moderate, and the lithium salt can be fully dissolved in the organic solvent, thereby reducing the probability of affecting the performance of the electrolyte due to deposition.
[0027] In one embodiment, the electrolyte consists of lithium salt and an organic solvent.
[0028] In the present application, the lithium salt and organic solvent contained in the electrolyte can meet the demand for fast charging of the battery without adding additional additives, which can save costs and reduce the probability of additives interacting with organic solvents, lithium salts, etc. to generate adverse by-products. At the same time, there are many types of additives, and the costs of screening and trial and error are high.
[0029] In some embodiments, the organic solvent includes one or more of linear carbonates and their substitutes, propylene carbonate (PC) and their substitutes, ethylene carbonate and their substitutes, linear carboxylates and their substitutes, nitriles and their substitutes, and sulfites and their substitutes. In this way, the requirements of fast-charge electrolyte for viscosity and dielectric constant can be met.
[0030] In some embodiments, the organic solvent includes at least one of ethylene carbonate and its substitutes, and at least one of nitriles and their substitutes.
[0031] In some embodiments, the organic solvent includes acetonitrile (AN) and fluoroethylene carbonate (FEC).
[0032] In the present application, acetonitrile has the characteristics of low viscosity, low melting point and high dielectric constant, which can improve the fast charging performance of the electrolyte; fluoroethylene carbonate is a good film-forming solvent, which is conducive to the formation of a LiF-rich and stable SEI film layer. The use of the two together can improve the fast charging performance of the electrolyte; at the same time, the two have similar solvation energies and can effectively participate in the solvation sheath, so that fluoroethylene carbonate and acetonitrile are preferentially combined, thereby reducing the probability of acetonitrile being embedded in the electrode material graphite and causing the graphite layer to be destroyed, thereby reducing the probability of causing the battery cycle life to decrease. The electrolyte of the present application has a high ionic conductivity in the temperature range of -30 to 60 ° C, and has good thermal stability, thereby improving the cycle stability of the battery under high-rate charge and discharge, and at the same time has a high ion transport capacity, which lays the foundation for improving the fast charging performance of lithium-ion batteries.
[0033] In some embodiments, the mass ratio of the acetonitrile to the fluoroethylene carbonate is (0.1-5):(5-10).
[0034] In this application, due to Li + In acetonitrile, it will be irreversibly embedded in the electrode material graphite. FEC has similar solvation energy to AN and can effectively participate in the solvation sheath, thereby reducing the AN and Li + The probability of embedding in graphite can be effectively controlled by controlling the mass ratio of acetonitrile and fluoroethylene carbonate. + The amount of Li embedded in graphite reduces +The irreversible loss of acetonitrile is reduced, and the probability of acetonitrile affecting the stability of the SEI film is reduced. At the same time, a sufficient number of free AN molecules is ensured in the solvation environment, thereby ensuring that the electrolyte has a high ionic conductivity, thereby improving the fast charging potential of the electrolyte.
[0035] In some embodiments, the mass ratio of the acetonitrile to the fluoroethylene carbonate is 3:7.
[0036] In this application, when the FEC / AN ratio is lower than 7 / 3, the amount of AN entering the solvation structure increases, which will hinder the formation of a dense and strong SEI film. + Will embed into graphite, causing Li + Irreversible loss reduces the battery capacity and causes a decrease in the battery cycle life; when the FEC / AN ratio is higher than 7 / 3, the number of free AN molecules in the solvation environment is insufficient, which reduces the ionic conductivity of the electrolyte and thus reduces the fast charging potential of the electrolyte.
[0037] In some embodiments, the lithium salt includes one or more of an inorganic lithium salt and an organic lithium salt.
[0038] In some embodiments, the inorganic lithium salt includes one or more of lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6) and lithium hexafluorophosphate (LiPF6).
[0039] In the present application, the above-mentioned lithium salts are maturely developed, have high purity, good solubility and high conductivity, and provide a basis for the electrolyte ions to achieve high conductivity.
[0040] In some embodiments, the organic lithium salt includes one or more of lithium bis(oxalatoborate) (LiBOB), lithium difluorooxalatoborate (LiDFOB), lithium bis(difluorosulfonyl)imide (LiFSI), and lithium bis(trifluoromethylsulfonyl)imide (LiTFSI).
[0041] In the present application, the above-mentioned lithium salts are maturely developed, have high purity, good solubility and high conductivity, and provide a basis for the electrolyte ions to achieve high conductivity.
[0042] In a second aspect, an embodiment of the present application provides a battery, comprising the above-mentioned electrolyte.
[0043] Example 1
[0044] An electrolyte and a preparation method thereof, comprising the following steps:
[0045] After removing water from acetonitrile (AN) with molecular sieves, it was mixed with fluoroethylene carbonate (FEC) at a mass ratio of 1:9. LiPF6 was weighed in a high-purity argon glove box and dissolved in fluoroethylene carbonate (FEC) and acetonitrile (AN) at a molar concentration of 1 mol / L. It was stirred overnight with a magnetic stirrer until it was completely dissolved and stored in a high-purity argon glove box for later use to obtain an electrolyte.
[0046] Example 2
[0047] This embodiment is substantially the same as Embodiment 1, except that the mass ratio of fluoroethylene carbonate (FEC) to acetonitrile (AN) in this embodiment is 8:2.
[0048] Example 3
[0049] This embodiment is substantially the same as Embodiment 1, except that the mass ratio of fluoroethylene carbonate (FEC) to acetonitrile (AN) in this embodiment is 7:3.
[0050] Example 4
[0051] This embodiment is substantially the same as Embodiment 1, except that the mass ratio of fluoroethylene carbonate (FEC) to acetonitrile (AN) in this embodiment is 6:4.
[0052] Example 5
[0053] This embodiment is substantially the same as Embodiment 1, except that the mass ratio of fluoroethylene carbonate (FEC) to acetonitrile (AN) in this embodiment is 5:5.
[0054] Example 6
[0055] This embodiment is substantially the same as Embodiment 1, except that fluoroethylene carbonate (FEC) is replaced by ethylene carbonate (EC) in this embodiment.
[0056] Example 7
[0057] This embodiment is substantially the same as Embodiment 1, except that in this embodiment, fluoroethylene carbonate (FEC) is replaced by diethyl carbonate (DEC).
[0058] Example 8
[0059] This embodiment is substantially the same as Embodiment 2, except that acetonitrile (AN) is replaced by succinonitrile (SN) in this embodiment.
[0060] Example 9
[0061] This embodiment is substantially the same as Embodiment 2, except that acetonitrile (AN) is replaced by adiponitrile (ADN) in this embodiment.
[0062] Example 10
[0063] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, fluoroethylene carbonate (FEC) is replaced by ethylene carbonate (EC) and dimethyl carbonate (DMC), wherein the volume ratio of ethylene carbonate (EC) to dimethyl carbonate (DMC) is 3:7.
[0064] Embodiment 11
[0065] This embodiment is substantially the same as Embodiment 1, except that acetonitrile (AN) is not used in this embodiment.
[0066] Example 12
[0067] This embodiment is substantially the same as Embodiment 2, except that the mass ratio of fluoroethylene carbonate (FEC) to acetonitrile (AN) in this embodiment is 3:7.
[0068] Comparative Example 1
[0069] This comparative example is substantially the same as Example 5, except that diethyl carbonate (DEC) and tetramethylsilane (TMS) are used to replace fluoroethylene carbonate (FEC) and acetonitrile (AN), and the mass ratio is still 5:5.
[0070] Test example:
[0071] Viscosity test: At a constant temperature (25±0.1°C), 100 ml of the prepared electrolyte of the embodiment and the comparative example was injected into a beaker, and the rotor of the rotary viscometer was immersed in the electrolyte to be tested for measurement to obtain the viscosity of each electrolyte at 25°C. The results are shown in Table 1.
[0072] Dielectric constant test: 50 ml of the prepared electrolytes of the embodiment and the comparative example were injected into the three-electrode cylindrical capacitor test box, and the capacitance value C of each electrolyte was measured. The dielectric constant ε of each electrolyte was calculated according to formula 1. The results are shown in Table 1. Where C0 and ε0 are respectively the capacitance of the three-electrode cylindrical capacitor test box (its structure is as shown in FIG. Figure 2 The capacitance value and dielectric constant value of the three-electrode cylindrical capacitor are shown in FIG. 1 ; L is the height of the electrolyte injected into the capacitor; D2 and D1 represent the diameters of the outer circle and inner circle of the three-electrode cylindrical capacitor respectively.
[0073]
[0074] Ionic conductivity: 5 ml of the prepared electrolyte of the embodiment and the comparative example was injected into a polytetrafluoroethylene reagent bottle, and the conductivity electrode was inserted and placed in a high and low temperature test box. The test temperature range was: -30 to 60°C, and the measurement was performed every 10°C. At the temperature to be measured, the electrolyte was left to stand for 0.5 to 1 hour, and then measured with a conductivity meter to obtain the conductivity values of the electrolyte in the temperature range of -30 to 60°C. The results are shown in Table 1 and Figure 1 shown.
[0075] Cyclic performance test: In a high-purity argon glove box, the electrolytes prepared in the examples and comparative examples were loaded into NCM811 / / graphite full cells, where NCM811 was used as the positive electrode (electrode load gram capacity: 0.45 mAh / cm 2 ), PE as a separator, 100 μL of the electrolyte of the embodiment and the comparative example is added, and finally graphite is used as the negative electrode to assemble the NCM811 / / graphite full battery. The cycle performance of the assembled NCM811 / / graphite full battery was tested using the CT2001A blue battery test system. The test conditions were: a high-rate cycle test at room temperature was performed at a charge and discharge rate of 1C, 5C, 8C, and 15C in the voltage range of 2.8V to 4.4V at 25°C. The test results are shown in Table 1.
[0076] Table 1 Cycling performance of NCM811 / / graphite full cells with different solvent system electrolytes
[0077]
[0078]
[0079] As can be seen from Table 1, compared with Example 10, the batteries of Examples 1-9 have significantly higher capacity retention rates at charge and discharge rates of 5C, 8C, and 15C, and significantly higher initial capacities at charge and discharge rates of 8C and 15C. It can be seen that the electrolytes of Examples 1-9 can improve the rate capability of the battery and enhance the fast charging performance of the battery. Compared with Examples 11 and 12, the batteries of Examples 1-5 have significantly higher capacity retention rates at charge and discharge rates of 5C, 8C, and 15C, and significantly higher initial capacities at charge and discharge rates of 15C. It can be seen that the ratio of FEC / AN in the electrolyte affects the rate capability and fast charging performance of the battery. Compared with Comparative Example 1, the batteries of the embodiment have significantly higher capacity retention rates and significantly higher initial capacities at charge and discharge rates of 1C, 5C, 8C, and 15C. It can be seen that the embodiment can improve the rate capability and fast charging performance of the battery by controlling the viscosity and / or dielectric constant of the organic solvent in the electrolyte.
[0080] Table 2 Conductivity values of different solvent system electrolyte solutions at different temperatures (unit: mS / cm)
[0081]
[0082]
[0083] From Table 2 and Figure 1 It can be seen that compared with Example 10 and Example 11, the electrolyte of Example 1 has higher ionic conductivity in the temperature range of -30 to 60° C. Although the electrolyte in Example 12 has higher ionic conductivity, when adapted to the battery, due to the high AN content in the electrolyte, it will cause graphite clogging, thereby causing the battery performance to deteriorate.
[0084] The embodiments of the present invention are described in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. At the same time, for those skilled in the art, according to the idea of the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present invention.
Claims
1. An electrolyte, It is characterized in that The invention comprises a lithium salt and an organic solvent, wherein the viscosity η of the organic solvent is less than 2.5 cp and / or the dielectric constant ε of the organic solvent is greater than 30.
2. The electrolyte according to claim 1, It is characterized in that The viscosity η of the organic solvent is less than 2.3 cp and / or the dielectric constant ε of the organic solvent is greater than 35; and / or The electrolyte consists of lithium salt and organic solvent.
3. The electrolyte according to claim 1, It is characterized in that The concentration of the lithium salt in the electrolyte is 0.1 to 4.0 mol / L.
4. The electrolyte according to claim 1, It is characterized in that The organic solvent includes one or more of linear carbonates and their substitutes, propylene carbonate and their substitutes, ethylene carbonate and their substitutes, linear carboxylates and their substitutes, nitriles and their substitutes, and sulfites and their substitutes.
5. The electrolyte according to claim 1, It is characterized in that The organic solvent includes at least one of ethylene carbonate and its substitutes, and at least one of nitriles and their substitutes.
6. The electrolyte according to claim 1, It is characterized in that The organic solvent includes acetonitrile and fluoroethylene carbonate.
7. The electrolyte according to claim 6, It is characterized in that The mass ratio of the acetonitrile to the fluoroethylene carbonate is (0.1-5):(5-10).
8. The electrolyte according to claim 6, It is characterized in that The mass ratio of the acetonitrile to the fluoroethylene carbonate is 3:
7.
9. The electrolyte according to claim 1, It is characterized in that The lithium salt includes one or more of an inorganic lithium salt and an organic lithium salt. The inorganic lithium salt includes one or more of lithium perchlorate, lithium tetrafluoroborate, lithium hexafluoroarsenate and lithium hexafluorophosphate. The organic lithium salt includes one or more of lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium bis(difluorosulfonylimide) and lithium bis(trifluoromethylsulfonylimide).
10. A battery, It is characterized in that Comprising the electrolyte as described in any one of claims 1-9.
Citation Information
Cited By
Lithium battery charging and discharging acceleration method based on lithium battery electrolyte proportion adjustment
CN120149600A
A lithium battery charging and discharging acceleration method based on lithium battery electrolyte proportioning adjustment