Preparation method and application of ultra-small grain full-coverage infrared perovskite thin film
Patent Information
- Application Number
- CN202411173747.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
AI Technical Summary
Existing near-infrared perovskite LEDs suffer from the contradiction of low efficiency at high brightness and low brightness at high efficiency, and their light extraction efficiency is limited. Traditional large-grain LEDs result in poor binding effect of photogenerated carriers, making it difficult to achieve efficient and stable light emission.
By adding additives to the perovskite precursor to regulate grain growth kinetics and using gradient annealing, small-grain perovskite thin films are prepared. Combined with appropriate electron and hole transport layer design, high-efficiency perovskite light-emitting diodes are formed.
This invention achieves high efficiency and high brightness perovskite light-emitting diodes, improves carrier mobility and stability, reduces crystal defects, extends device lifespan, and enhances light extraction efficiency.
Smart Images

Figure CN119053211A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of display lighting, and in particular to a preparation method of a near-infrared perovskite film with ultra-small crystal grains and application thereof. Background Art
[0002] The unique soft lattice of perovskite materials has the characteristics of high defect tolerance. Because of this, polycrystalline films have been developed into high-efficiency luminescent materials comparable to traditional quantum dots (QDs). Although perovskite light-emitting diodes (PeLEDs) have made significant progress in performance, the morphology and structural defects of perovskites still limit the injection and recombination of carriers. For example, polycrystalline films with a size of hundreds of nanometers provide a wide space for the diffusion of carriers, allowing carriers to move freely in a large range, but at the same time, it also greatly increases the probability of carriers being captured by various defects, such as point defects and high-dimensional defects (such as domain boundaries, edge dislocations, etc.). Although pre-synthesized quantum dots can solve the problem of insufficient radiative recombination by enhancing the confined space, in actual device applications, the long-chain ligands at the interface of adjacent quantum dots in the quantum dot luminescent film stacked by multiple quantum dots are likely to become potential transmission loss traps, which inhibit the recombination and transmission of carriers.
[0003] Most of the near-infrared perovskite LEDs reported so far often have the contradiction of too low efficiency at high brightness and too low brightness at high efficiency. How to maintain high efficiency and high stability at high brightness is an important problem faced by this field and a key technical bottleneck restricting its commercial application. For example, to achieve high brightness, it may be necessary to increase the current density, but this may lead to increased heat generation, thus affecting the stability and efficiency of the device. In addition, the external quantum efficiency of perovskite LEDs depends on the "light extraction efficiency" or "external coupling efficiency" determined by the optical design of the device. For infrared perovskite LEDs, the high refractive index may be one of the key reasons why photons are difficult to emit, which limits the improvement of light extraction efficiency. Although some materials with similar treatment methods to perovskites but lower refractive index can be used to reduce the refractive index of the light-emitting layer, the adjustment range is relatively limited. In addition, the size of traditional large grains is large, which makes it poorly bound to photogenerated carriers. In this case, photogenerated carriers are easy to escape and difficult to be effectively confined inside the grains, resulting in limited luminescence performance. Summary of the invention
[0004] The present invention provides a method for preparing a perovskite film with ultra-small crystal grains, wherein an additive is added to a perovskite precursor to adjust the growth dynamics of the perovskite crystal grains, and a perovskite film with small crystal grains is obtained by a gradient annealing method to realize a high-efficiency PeLED, and the method comprises the following steps:
[0005] S1: Preparation of perovskite precursor solution
[0006] A certain amount of monovalent cation salt, lead halide and additives are added to a certain amount of N,N-dimethylformamide solution, and then placed in a glove box in a nitrogen environment. The solution is stirred for a certain period of time at a certain temperature and a certain rotation speed. The temperature of the mixed solution is then increased, and the solution is stirred for a certain period of time at a certain rotation speed in the glove box in a nitrogen environment to obtain a clear and transparent perovskite precursor solution.
[0007] S2: Preparation of electron transport layer
[0008] A clean transparent conductive substrate is selected, and the transparent conductive substrate is treated with ultraviolet ozone or plasma for 15 to 30 minutes. Then, a certain amount of metal oxide solution is prepared on the conductive substrate by a spin coating process, and then the conductive substrate is transferred to a hot stage and annealed for a certain time and temperature. Then, a layer of PEIE is spin-coated, and then annealed again to obtain an electron transport layer.
[0009] S3: Obtaining small grains fully covered perovskite film
[0010] The electron transport layer obtained by S2 is placed in a glove box in a nitrogen environment, and then a certain amount of perovskite precursor solution is spin-coated on the electron transport layer at a certain rotation speed, and then annealed three times on a hot stage to form a small grain-fully covered perovskite film on the substrate.
[0011] Further, in S1, the monovalent cation salt is one or more of formamidine hydroiodide (FAI), methylamine iodide (MAI), 2-phenylethylamine hydroiodide (PEAI), cesium iodide (CsI), cesium bromide (CsBr), cesium chloride (CsCl) and cesium fluoride (C); the lead halide is one or more of lead iodide, lead bromide, lead chloride and lead fluoride; the additive is thiobetaine iodine, 5-aminovaleric acid, 5-2-aminobenzophenone-2'-carboxylic acid, 2,2-iminodibenzoic acid, 3-aminopropionic acid, 4-aminobutyric acid, 5-aminohexanoic acid, 6-aminoheptanoic acid, 4-amino-3-hydroxybutyric acid, 2-aminocyclopentanecarboxylic acid, 3-aminocyclohexanecarboxylic acid, 4-aminophenylacetic acid, 3-amino One or more of phenylpropionic acid, 2-amino-1,5-phthalic acid, 3-amino-1,4-phthalic acid, 4-amino-1,4-phthalic acid, 2-amino-2-methylpropionic acid, 3-amino-2-ethylbutyric acid, 4-aminophenylacetamide-4'-carboxylic acid, 3-aminophenylbutyramide-3'-carboxylic acid, 2-aminobenzaldehyde acid, and 5-aminophenylbutyraldehyde acid; the specific temperature is 50-80° C., the stirring speed is 200 rpm-800 rpm, and the stirring time is 1 to 4 hours; the temperature after the increase is 60-120° C., after heating, the stirring speed is 300 rpm-500 rpm, and the stirring time is 0.5 to 14 hours; the concentration of the precursor solution is 0.0012-1.1731 g / mL.
[0012] Further, in S2, the transparent conductive substrate is a rigid indium tin oxide (ITO) transparent conductive film glass, fluorine tin oxide (FTO) transparent conductive film glass or aluminum zinc oxide (AZO) transparent conductive film glass; the metal oxide solution is one of tin oxide (SnO2), zinc oxide (ZnO), titanium oxide (TiO2), and ZnMgO. The amount of metal oxide added is 30-80 μL, the spin coating time is 20-60s, and the spin coating speed is 2000-5000rpm; the annealing temperature is 50-300℃, and the annealing time is 5min-120min; the spin coating time of PEIE is 20-60s, the spin coating speed is 2000-8000rpm, and the annealing temperature after spin coating PEIE is 50-200℃, and the annealing time is 5min-90min.
[0013] Further, in S3, the amount of the perovskite precursor solution added is 30-80 μL, the spin coating time is 20-60 s, the spin coating speed is 2000-5000 rpm, the first annealing temperature is 30-50°C, and the annealing time is 30s-20min; the second annealing temperature is 50-80°C, and the annealing time is 20s-15min; the third annealing temperature is 80-140°C, and the annealing time is 30s-30min.
[0014] A small-grain fully covered perovskite film is prepared by the above method.
[0015] An infrared perovskite LED device is obtained by spin coating a certain substance on the top of a perovskite film that fully covers small grains, then performing an annealing treatment to form an organic hole transport layer or an inorganic hole transport layer, vapor-depositing an interface modification layer on the organic hole transport layer or the inorganic hole transport layer, and vapor-depositing a layer of electrode on the interface modification layer to obtain an LED device.
[0016] Further, the organic hole transport layer is poly(3-hexylthiophene-2,5-diyl) (P3HT), poly[(9,9-dioctylfluorene-2,7-diyl)-co-(4,4′-(N-(4-sec-butylphenyl)diphenylamine)] (TFB), [bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA), poly[[4,8-bis[(2-ethylhexyl)oxy]-benzo[1,2-B:4,5-B′]dithiophene-2,6-diyl][3-fluoro-2-[(2-ethylhexyl)carbonyl]thiophene[3,4-b]thiophene] (PTBT), poly[bis(4-phenyl)(4-butylphenyl)amine] (Poly-TPD) or 2,2′,7,7′-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9 '-Spiro-OMeTAD; the inorganic hole transport layer is nickel oxide (NiO), vanadium pentoxide (V2O5), tungsten oxide (WO), cuprous oxide (Cu2O) or cuprous thiocyanate (CuSCN); the spin coating time is 20-60s, the spin coating speed is 2000-5000rpm, the annealing temperature is 30-50℃, and the annealing time is 30s-5min; the interface modification layer is one or more of bathocuproine (BCP), lithium fluoride (LiF), cesium carbonate, molybdenum oxide (MoO3), polymethyl methacrylate or 8-hydroxyquinoline aluminum (Alq3); the thickness of the interface modification layer is 1-10nm, the electrode is one or more of nickel, titanium, calcium, aluminum, copper, silver, gold, carbon or graphene electrode, and the vacuum degree during evaporation is 3.8×10 -6 ~7.3×10 -4 Pa, the evaporation rate is 0.001-0.08nm / s, and the electrode thickness is 30-120nm.
[0017] Advantages of the present invention:
[0018] 1. By adding additives to the perovskite precursor, the crystallization process of perovskite can be regulated to make the crystal more uniform and dense and reduce crystal defects. For example, some organic small molecule additives can interact with the ions in the perovskite to guide the orderly growth of the crystal, thereby improving the crystallization quality of the perovskite film. This helps to reduce non-radiative recombination centers, improve carrier mobility and lifetime, and thus improve the performance of perovskite devices, while enhancing stability to water, oxygen and heat: certain additives can form a protective film on the surface of the perovskite to prevent the intrusion of water and oxygen, thereby improving the stability of the perovskite film in the air. At the same time, some additives can also improve the thermal stability of the perovskite, so that it can still maintain good performance at higher temperatures. In addition, additives can form stable complexes with the ions in the perovskite, reduce ion migration, and thus improve the stability and life of the device.
[0019] 2. By spin coating a certain amount of metal oxide on the conductive substrate, the perovskite layer is prevented from directly contacting the electrode, providing a certain mechanical support and stability for the device, protecting sensitive functional layers such as the light-emitting layer from external environmental factors (such as oxygen, water vapor, etc.), and extending the service life of the QLED device. At the same time, electrons are mainly efficiently transferred from the electrode to the light-emitting layer, while preventing the holes in the light-emitting layer from being reversely transferred to the electrode or other functional layers, avoiding the recombination of electrons and holes in the non-light-emitting area, thereby improving the recombination efficiency of electrons and holes in the light-emitting layer, for example, the recombination efficiency can be increased by a certain percentage.
[0020] 3. In S3, a gradient annealing method can be used to promote the formation of a more regular structure of perovskite crystals, reduce crystal defects, and improve key electrical performance parameters such as carrier mobility. For example, the carrier mobility can be increased by a certain percentage, while helping to obtain a smoother film surface, reducing surface roughness, facilitating the preparation and good contact of subsequent electron transport layers or electrodes, and improving the performance stability of the device. The surface roughness can be reduced by several nanometers. More importantly, gradient annealing can guide the growth of perovskite crystals in a specific direction and optimize its photoelectric performance. In addition, a proper gradient annealing process can reduce the stress inside the film, enhance its resistance to environmental factors (such as humidity, oxygen, etc.), and extend the service life of the perovskite device.
[0021] 4. The small-grain perovskite light-emitting layer of the present invention, by virtue of its smaller grain size, can better bind photogenerated carriers. This advantage enables the carriers to exist more stably inside the grains, achieving more efficient luminescence performance. Compared with pre-synthesized quantum dots, although quantum dots can solve the problem of insufficient radiation recombination by enhancing the confined space, in practical applications, the long-chain ligands at the interface of adjacent quantum dots in the quantum dot light-emitting film stacked by multiple quantum dots are likely to become potential transmission loss traps, which inhibit the recombination and transmission of carriers. The ultra-small-grain perovskite layer prepared by the present invention effectively avoids this problem, provides an excellent recombination and transmission environment for carriers, greatly improves the overall performance of infrared perovskite LED devices, has broad application prospects and significant market value, and is expected to trigger major changes in related fields and promote industrial development.
[0022] 5. LED devices have high device efficiency and high irradiance, and can still maintain a high irradiance and efficiency at high current density. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A scanning electron microscope photograph of a perovskite film obtained according to a method for preparing a near-infrared perovskite film with ultra-small crystal grains and application in LEDs of the present invention;
[0024] Figure 2 The X-ray diffraction curve diagram of the perovskite film obtained according to the preparation method of the near-infrared perovskite film with ultra-small crystal grains and the application in LED of the present invention;
[0025] Figure 3 A fluorescence spectrum curve of a perovskite film obtained according to a method for preparing a near-infrared perovskite film with ultra-small crystal grains and an application in an LED of the present invention;
[0026] Figure 4 The ultraviolet-visible absorption spectrum of the perovskite film obtained by the preparation method of the near-infrared perovskite film with ultra-small crystal grains and the application in LED according to the present invention;
[0027] Figure 5 The present invention provides a method for preparing a near-infrared perovskite film with ultra-small crystal grains and a curve showing a change in irradiance of a near-infrared LED device with driving voltage obtained by using the method in the present invention. Figure 6 The irradiance variation curve of an infrared perovskite LED device with respect to voltage is obtained according to a method for preparing a near-infrared perovskite film with ultra-small crystal grains of the present invention and an application in LED. DETAILED DESCRIPTION
[0028] The present invention will be further described below through specific embodiments in conjunction with the accompanying drawings.
[0029] Example 1
[0030] A method for preparing a perovskite film with ultra-small grains comprises the following steps:
[0031] S1. 0.0447 g of formamidine hydroiodide (FAI), 0.0599 g of lead iodide (PbI2) and 0.0118 g of 5-aminocaproic acid were added to 1 mL of N,N-dimethylformamide, placed in a glove box in a nitrogen environment, stirred at 200 rpm for 4 h at 50 ° C, then the mixed solution was heated to 70 ° C, and then continued to stir at 300 rpm for 16 h in a glove box in a nitrogen environment to obtain a clear and transparent perovskite precursor solution of 0.1194 g / mL;
[0032] S2. Select clean aluminum zinc oxide (AZO) transparent conductive film glass, treat the aluminum zinc oxide (AZO) transparent conductive film glass with ultraviolet ozone or plasma for 15 minutes, and then prepare a certain amount of ZnMgO solution on the transparent conductive film glass by spin coating process, the spin coating speed is 2000 rpm, the spin time is 20 seconds, and then the transparent conductive film glass is transferred to a hot stage, annealed at 150°C for 15 minutes, and then spin coated with a layer of PEIE, the spin coating speed is 5000 rpm, the spin coating time is 50 seconds, and then annealed at 100°C for 90 minutes to obtain an electron transport layer;
[0033] S3. Place the electron transport layer obtained in S2 into a glove box with a nitrogen environment, and then spin-coat 30 μL of the perovskite precursor solution on the electron transport layer at a speed of 4000 rpm for 30 seconds. After the spin coating, immediately transfer the sample to a hot stage, and anneal it at 50°C for 5 minutes, then at 80°C for 5 minutes, and then at 105°C for 8 minutes. After cooling to room temperature, a perovskite film fully covered with small grains is obtained.
[0034] Through SEM characterization of the perovskite film, it was found that the perovskite film was fully covered and the grain size was about 30-80nm ( Figure 1 ), and then the perovskite film was characterized by XRD, and it was found that the perovskite film had strong diffraction peaks at 14.22° and 28.51°, indicating that the perovskite has strong crystallinity ( Figure 2 ). Steady-state fluorescence characterization of perovskite film revealed that the fluorescence peak of the perovskite film is at 803nm, and the half-peak width is about 50nm ( Figure 3 ), and through the characterization of ultraviolet absorption, it was found that the ultraviolet absorption peak of the perovskite film is around 780nm ( Figure 4 ).
[0035] Example 2
[0036] A method for preparing a perovskite film with ultra-small grains comprises the following steps:
[0037] S1. Add 0.0403 g of formamidine hydroiodide (FAI), 0.0041 g of methylammonium iodide (MAI), 0.0476 g of lead iodide (PbI2) and 0.0076 g of 5-aminohexanoic acid into 1 mL of N,N-dimethylformamide, put into a glove box in a nitrogen environment, stir at 400 rpm for 3 h at 70 ° C, then heat the mixed solution to 90 ° C, and then continue to stir at 400 rpm for 20 h in a glove box in a nitrogen environment to obtain a clear and transparent perovskite precursor solution of 0.0920 g / mL;
[0038] S2. Select clean indium tin oxide (ITO) transparent conductive film glass, treat the indium tin oxide (ITO) transparent conductive film glass with ultraviolet ozone or plasma for 20 minutes, and then prepare a certain amount of tin oxide (SnO2) solution on the transparent conductive film glass by spin coating process, the spin coating speed is 3000 rpm, the spin time is 40 seconds, and then transfer the transparent conductive film glass to a hot stage, anneal at 120°C for 30 minutes, and then spin coat a layer of PEIE, the spin coating speed is 5000 rpm, the spin coating time is 50 seconds, and then anneal at 150°C for 30 minutes to obtain an electron transport layer;
[0039] S3. Place the electron transport layer obtained in S2 into a glove box with a nitrogen environment, and then spin-coat 50 μL of the perovskite precursor solution on the electron transport layer at a speed of 4000 rpm for 30 seconds. After the spin coating is completed, immediately transfer the sample to a hot stage, first anneal at 40°C for 10 minutes, then anneal at 70°C for 10 minutes, and then anneal at 120°C for 20 minutes. After cooling to room temperature, a perovskite film fully covered with small grains is obtained.
[0040] Example 3
[0041] A method for preparing a perovskite film with ultra-small grains comprises the following steps:
[0042] S1. 0.0403 g of formamidine hydroiodide (FAI), 0.0067 g of cesium iodide (CsI), 0.0599 g of lead iodide (PbI2), and 0.0080 g of thiobetaine were added to 1 mL of N,N-dimethylformamide, placed in a nitrogen environment glove box, stirred at 800 rpm for 1 h at 80 ° C, then the mixed solution was heated to 120 ° C, and then continued to stir at 500 rpm for 2 h in a nitrogen environment glove box to obtain a clear and transparent perovskite precursor solution of 0.1149 g / mL;
[0043] S2. Select clean fluorine tin oxide (FTO) transparent conductive film glass, treat the fluorine tin oxide (FTO) transparent conductive film glass with ultraviolet ozone or plasma for 30 minutes, and then prepare a certain amount of titanium oxide (TiO2) solution on the transparent conductive film glass by spin coating process, the spin coating speed is 5000 rpm, the spin time is 60 seconds, and then the transparent conductive film glass is transferred to a hot stage, annealed at 300°C for 120 minutes, and then spin coated with a layer of PEIE, the spin coating speed is 8000 rpm, the spin coating time is 60 seconds, and then annealed at 200°C for 50 minutes to obtain an electron transport layer;
[0044] S3. Place the electron transport layer obtained in S2 into a glove box with a nitrogen environment, and then spin-coat 80 μL of the perovskite precursor solution on the electron transport layer at a speed of 5000 rpm for 60 seconds. After the spin coating, immediately transfer the sample to a hot stage, and anneal it at 50°C for 20 minutes, then at 80°C for 15 minutes, and then at 140°C for 30 minutes. After cooling to room temperature, a perovskite film fully covered with small grains is obtained.
[0045] Example 4
[0046] The top of the perovskite film fully covered with small grains obtained in Example 1 was spin-coated with poly [[4,8-bis[(2-ethylhexyl)oxy]-benzo[1,2-B:4,5-B']dithiophene-2,6-diyl][3-fluoro-2-[(2-ethylhexyl)carbonyl]thiophene[3,4-b]thiophene] (PTBT), with a spin coating speed of 2000 rpm and a rotation time of 20 s; then annealed at 30°C for 40 s, thereby preparing a hole transport layer on the top of the perovskite film fully covered with small grains, and then 5 nm of MoO3 was evaporated on the top hole transport layer as an interface modification layer, and then 100 nm of gold was evaporated on the interface modification layer as an electrode, thereby obtaining an infrared perovskite LED device.
[0047] The performance of the prepared LED device was characterized and it was found that the near-infrared perovskite LED we prepared achieved an efficiency close to 20% ( Figure 5 ) and the maximum irradiance reached 314W sr -1 m -2 ( Figure 6 ).
[0048] Example 5
[0049] The top of the perovskite film fully covered with small grains obtained in Example 2 was spin-coated with poly [[4,8-bis[(2-ethylhexyl)oxy]-benzo[1,2-B:4,5-B']dithiophene-2,6-diyl][3-fluoro-2-[(2-ethylhexyl)carbonyl]thiophene[3,4-b]thiophene] (PTBT), with a spin coating speed of 4000 rpm and a rotation time of 40 s; then annealed at 40°C for 1 min, thereby preparing a hole transport layer on the top of the perovskite film fully covered with small grains, and then 3 nm of MoO3 was evaporated on the top hole transport layer as an interface modification layer, and then 100 nm of gold was evaporated on the interface modification layer as an electrode, thereby obtaining an infrared perovskite LED device.
[0050] Example 6
[0051] The top of the perovskite film fully covered with small grains obtained in Example 3 was spin-coated with poly [[4,8-bis[(2-ethylhexyl)oxy]-benzo[1,2-B:4,5-B']dithiophene-2,6-diyl][3-fluoro-2-[(2-ethylhexyl)carbonyl]thiophene[3,4-b]thiophene] (PTBT), with a spin coating speed of 5000 rpm and a rotation time of 60 s; then annealed at 50°C for 4 min, thereby preparing a hole transport layer on the top of the perovskite film fully covered with small grains, and then 3 nm of MoO3 was evaporated on the top hole transport layer as an interface modification layer, and then 100 nm of gold was evaporated on the interface modification layer as an electrode, thereby obtaining an infrared perovskite LED device.
[0052] Finally, it should be noted that the purpose of publishing the embodiments is to help further understand the present invention, but those skilled in the art can understand that various substitutions and modifications are possible without departing from the spirit and scope of the present invention and the appended claims. Therefore, the present invention should not be limited to the contents disclosed in the embodiments, and the scope of protection claimed by the present invention shall be subject to the scope defined in the claims.
Claims
1. A method for preparing a perovskite film with ultra-small grains, characterized in that: The following steps are involved: S1: preparing perovskite precursor solution; S2: preparing electron transport layer; S3: Obtaining small grains fully covered perovskite film; The electron transport layer obtained by S2 is placed in a glove box in a nitrogen environment, and then a certain amount of perovskite precursor solution is spin-coated on the electron transport layer at a certain rotation speed, and then annealed three times on a hot stage to form a small grain-fully covered perovskite film on the substrate.
2. A small-grain fully covered perovskite film, characterized in that: Prepared by the method of claim 1.
3. An infrared perovskite LED device, characterized in that: An LED device is obtained by spin coating a certain substance on the top of the small-grain fully covered perovskite film as described in claim 2, and then performing annealing to form an organic hole transport layer or an inorganic hole transport layer, evaporating an interface modification layer on the organic hole transport layer or the inorganic hole transport layer, and evaporating a layer of electrode on the interface modification layer.