Ultrathin core-shell structure photocatalyst as well as preparation method and application thereof
By using ultra-thin core-shell structure Ag@Au nanomaterials in photocatalysts, the dual plasmon field superposition resonance between the Ag core and the Au shell is solved, and the problem of low thermal carrier separation efficiency of traditional catalysts is significantly improved. Photocatalytic carbon dioxide reduction activity and methane-producing selectivity.
Patent Information
- Application Number
- CN202411247951.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-03
AI Technical Summary
The heat carrier separation efficiency of traditional single-component plasmon metal nanoparticle catalysts is low, which makes it difficult to efficiently utilize thermal electrons, limiting the significant improvement of photocatalytic carbon dioxide conversion activity.
Ultra-thin core-shell structure photocatalyst is composed of Ag nanocubes with side lengths of 18nm to 48nm and Au shell with average thickness of 1nm to 4nm. It is formed by polyol reduction method and photodeposition method. The double weight of Ag core and Au shell is The superposition of plasmon field resonance improves light absorption efficiency and promotes directional separation and rapid migration of hot carriers.
The photocatalytic carbon dioxide reduction activity was significantly improved, the methane production performance reached 867.36μmol h-1g-1, and the methane production selectivity was 93.61%, which was better than the pure Ag nanoparticle catalyst.
Smart Images

Figure CN119056445A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of photocatalysts, and in particular relates to an ultra-thin core-shell structure photocatalyst and a preparation method and application thereof. Background Art
[0002] How to seek green and clean energy and solve the current energy supply problem is a difficult problem facing people. Driven by sunlight, photocatalytic carbon dioxide reduction technology, which uses abundant carbon dioxide in the atmosphere and water from a wide range of sources as raw materials to synthesize hydrocarbon fuels, is considered to be a feasible solar-chemical energy conversion strategy. However, the activity of traditional photocatalysts in converting carbon dioxide to methane is less than 100 μmol h -1 g -1 The low conversion efficiency is the key bottleneck restricting its large-scale application.
[0003] In recent years, plasmonic nanostructured photocatalysts, due to their unique localized surface plasmon resonance characteristics, can not only greatly improve light absorption efficiency, but also accelerate the carbon dioxide conversion process by generating hot electrons. Traditional single-component plasmonic metal nanoparticle catalysts have poor hot carrier separation efficiency, which makes it difficult to efficiently extract and utilize the hot electrons they generate, limiting the significant improvement of their photocatalytic carbon dioxide conversion activity. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention provides an ultrathin core-shell structure photocatalyst. The novel hybrid bimetallic plasmon nano ultrathin core-shell structure catalyst solves the technical problems of low hot carrier separation efficiency and difficulty in efficient utilization of hot electrons existing in traditional single-component plasmon metal nanoparticle catalysts.
[0005] To achieve the above objectives, the present invention provides the following technical solutions:
[0006] An ultra-thin core-shell structure photocatalyst, which is a mixed bimetallic plasmon nanostructure material, consisting of Ag nanocubes with a side length of 18nm to 48nm and an Au shell with an average thickness of 1nm to 4nm.
[0007] Preferably, the mass ratio of Ag / Au of the photocatalyst is 0.45% to 3.80%.
[0008] Preferably, the photocatalyst is a hybrid bimetallic plasmon nanostructure material, consisting of Ag nanocubes with a side length of 30 nm and an Au shell with an average thickness of 1.5 nm, and the Ag / Au mass ratio of the photocatalyst is 1.6%.
[0009] A method for preparing an ultrathin core-shell structure photocatalyst, the method for preparing the photocatalyst comprising the following steps:
[0010] Step 1: Add 40 mL of DEG or EG into a 100 mL round-bottom single-necked flask, stir and heat in a 150 °C oil bath for 30 min;
[0011] Step 2: First, add 0.5 mL of NaSH solution with a molar concentration of 3 mM to 6 mM, then add 4 mL of HCl solution with a molar concentration of 3 mM after 4 minutes, then add 10 mL of PVP solution with a mass concentration of 20 mg / mL to 40 mg / mL after an interval of 4 minutes, and finally add 3 mL of CF3COOAg solution with a molar concentration of 280 mM. The prepared reagent solutions all use DEG or EG as solvent;
[0012] Step 3: Stir and heat the solution from step 2 in a 150°C oil bath for 30 to 480 min. During the entire process, except for adding reagents, the flask was sealed with a glass stopper;
[0013] Step 4: After the reaction is completed, the flask is immediately placed in an ice water bath for cooling and quenching, and then washed with acetone for precipitation and then washed with ultrapure water three times to obtain Ag nanocubes, which are then dispersed in ultrapure water and prepared into a 1.855 mg / mL Ag nanocube aqueous solution;
[0014] Step 5: Add 2.7 mL of the Ag nanocube aqueous solution obtained in step 4 and 35 μL to 432 μL of an AuCl4H aqueous solution with a mass concentration of 0.5 mg / mL to 100 mL of a methanol aqueous solution with a volume concentration of 10% vol, and mix well;
[0015] Step 6: The solution in step 5 was continuously stirred and irradiated under a 300 W xenon lamp for 1.5 h to 3 h for photodeposition. After washing the sample three times with ultrapure water, an ultrathin core-shell structure photocatalyst was obtained.
[0016] Preferably, the solvent in step 1 is DEG, and the molar concentration of the NaSH solution in step 2 is 3 mM.
[0017] Preferably, the mass concentration of the PVP solution in step 2 is 20 mg / mL.
[0018] Preferably, when the solvent in step 1 is DEG, the stirring and heating time in step 3 is 480 min.
[0019] Preferably, the volume of the AuCl4H aqueous solution added in step 5 is 173 μL.
[0020] Preferably, the photodeposition time in step six is 3 hours.
[0021] An ultrathin core-shell structure photocatalyst is applied to photocatalytic carbon dioxide reduction to produce methane, comprising the following steps:
[0022] Step 1: Disperse 5 mg of the ultrathin core-shell structure photocatalyst prepared in claim 1 in 6 mL of ultrapure water, perform ultrasonic dispersion, drop-coat on an aluminum foil substrate, and dry under vacuum at 60° C.
[0023] Step 2: Add 1.5 g of sodium bicarbonate to the bottom of the quartz reactor and place the aluminum foil substrate with the photocatalyst on the bracket;
[0024] Step 3: Connect and fix the quartz reactor to the all-glass automatic online trace gas analysis system, turn on the vacuum pump and plunger pump, evacuate the reaction device, inject high-purity argon gas into the quartz reactor to evacuate again, and repeat three times;
[0025] Step 4: Inject 10 mL of 0.8 M sulfuric acid into the bottom of the reactor to generate the carbon dioxide and water vapor required for the reaction, turn on the xenon lamp to react, and take samples every 20 minutes to measure the activity.
[0026] Compared with the prior art, the ultra-thin core-shell structure photocatalyst provided by the present invention has the following beneficial effects:
[0027] Ag and Au, two plasmonic metals, are combined by polyol reduction method and photodeposition method to form an ultrathin core-shell photocatalyst. Under light excitation conditions, the dual plasmon field formed by the Ag core and the Au shell superimposes and resonates on the surface of the catalyst nanostructure, which can significantly improve the light absorption efficiency of the catalyst and stimulate the generation of a large number of hot carriers. At the same time, the construction of the ultrathin core-shell structure can effectively promote the directional separation and rapid migration of hot carriers at the interface between the two, improve the utilization efficiency of hot electrons, and thus greatly improve the photocatalytic carbon dioxide reduction activity. This new Ag@Au photocatalyst with ultrathin core-shell structure has higher carbon dioxide reduction activity than pure Ag nanoparticle photocatalyst, and its methane production performance can reach 867.36μmol h -1 g -1 , the methane selectivity is 93.61%. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a scanning transmission electron microscope image of the catalyst of Example 1 of the present invention;
[0029] Figure 2 This is a comparison chart of the UV-visible diffuse reflectance spectrum test results of the catalyst of Example 1 of the present invention and pure Ag nanoparticles;
[0030] Figure 3 This is a comparison chart of the photocurrent response test results of the catalyst of Example 1 of the present invention and pure Ag nanoparticles;
[0031] Figure 4 This is a comparison chart of electrochemical impedance test results of the catalyst of Example 1 of the present invention and pure Ag nanoparticles;
[0032] Figure 5 This is a comparison chart of the methane production by carbon dioxide reduction of the catalyst of Example 1 of the present invention and pure Ag nanoparticles;
[0033] Figure 6 This is a comparison chart of carbon monoxide production from carbon dioxide reduction using the catalyst of Example 1 of the present invention and pure Ag nanoparticles. DETAILED DESCRIPTION
[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] It should be noted that:
[0036] DEG described in the present invention refers to: diethylene glycol;
[0037] The EG described in the present invention refers to: ethylene glycol;
[0038] The PVP described in the present invention refers to: polyvinyl pyrrolidone;
[0039] The mM mentioned in the present invention refers to millimole per liter.
[0040] Example 1
[0041] An ultra-thin core-shell structure photocatalyst and a preparation method thereof, the catalyst preparation method comprising the following steps:
[0042] Step 1: Add 40 mL of DEG into a 100 mL round-bottom single-necked flask, stir and heat in a 150 °C oil bath for 30 min;
[0043] Step 2: First, add 0.5 mL of NaSH solution with a molar concentration of 3 mM, then add 4 mL of HCl solution with a molar concentration of 3 mM after 4 minutes, then add 10 mL of PVP solution with a mass concentration of 20 mg / mL after an interval of 4 minutes, and finally add 3 mL of CF3COOAg solution with a molar concentration of 280 mM. The prepared reagent solutions all use DEG as solvent;
[0044] Step 3: The solution from step 2 was stirred and heated in an oil bath at 150°C for 480 min. During the entire process, except for the addition of reagents, the flask was sealed with a glass stopper;
[0045] Step 4: After the reaction is completed, the flask is immediately placed in an ice water bath for cooling and quenching, and then washed with acetone for precipitation and then washed with ultrapure water three times to obtain Ag nanocubes, which are then dispersed in ultrapure water and prepared into a 1.855 mg / mL Ag nanocube aqueous solution;
[0046] Step 5: Add 2.7 mL of the aqueous solution of Ag nanocubes obtained in step 4 and 173 μL of an aqueous solution of AuCl4H with a concentration of 0.5 mg / mL to 100 mL of an aqueous solution of methanol with a volume concentration of 10% vol. and mix well;
[0047] Step 6: The solution in step 5 was continuously stirred and irradiated for 3 h under a 300 W xenon lamp for photodeposition. After washing the sample three times with ultrapure water, an ultrathin core-shell structured Ag@Au photocatalyst was obtained.
[0048] The microstructure of the catalyst prepared in Example 1 was characterized by high-angle annular dark field scanning transmission electron microscopy (HAADF-STEM) and energy dispersive X-ray spectroscopy (EDX). Figure 1 The characterization results showed that the catalyst was composed of Ag nanocubes with a side length of 30 nm and an Au shell with an average thickness of 1.5 nm. Au was evenly distributed on the surface of the Ag nanocubes and completely covered them, proving that the Ag@Au photocatalyst with an ultra-thin core-shell structure was successfully constructed.
[0049] The element content in the catalyst prepared in Example 1 was measured by inductively coupled plasma mass spectrometry, and the measurement results showed that the Au / Ag mass ratio was 1.6%.
[0050] The light absorption performance of the prepared catalyst was compared with that of pure Ag nanoparticles by UV-visible diffuse reflectance spectroscopy. It was shown that the prepared catalyst has a significantly enhanced light absorption in the visible light region of 450nm to 800nm compared with pure Ag nanoparticles. Please refer to the attached Figure 2 .
[0051] Using photocurrent response, please refer to the attached Figure 3 and electrochemical impedance, please refer to the attached Figure 4 The electrochemical properties of the prepared catalyst were characterized, and the results showed that compared with pure Ag nanoparticles, the photocurrent intensity of the prepared catalyst increased by 2 times and the Nyquist circle radius decreased by 9 times, proving that the prepared catalyst has stronger hot carrier separation and migration efficiency.
[0052] The ultra-thin core-shell structure photocatalyst prepared in Example 1 is applied to photocatalytic carbon dioxide reduction to produce methane, comprising the following steps:
[0053] Step 1: Disperse 5 mg of ultrathin core-shell structured photocatalyst in 6 mL of ultrapure water, disperse by ultrasonication, drop-coat on an aluminum foil substrate, and dry under vacuum at 60 °C;
[0054] Step 2: Add 1.5 g of sodium bicarbonate to the bottom of the quartz reactor and place the aluminum foil substrate with the photocatalyst on the bracket;
[0055] Step 3: Connect and fix the quartz reactor to the Labsolor-6A all-glass automatic online trace gas analysis system, turn on the vacuum pump and plunger pump, evacuate the reaction device, inject high-purity argon gas into the quartz reactor and evacuate again, and repeat three times;
[0056] Step 4: 10 mL of 0.8 M sulfuric acid was injected into the bottom of the reactor to generate carbon dioxide and water vapor required for the reaction, and the xenon lamp was turned on for reaction. The reaction products were analyzed by gas chromatography automatic sampling system. The reaction results are listed in Table 1.
[0057] Please refer to the attached Figure 5 And attached Figure 6 , the photocatalyst prepared in Example 1 and pure Ag nanoparticles under simulated sunlight irradiation, the yield of carbon dioxide converted into methane and carbon monoxide changes with irradiation time. The prepared catalyst exhibits better photocatalytic carbon dioxide reduction methanogenesis activity than pure Ag nanoparticles, which is 2.5 times the methanogenesis performance of pure Ag nanoparticles, and the selectivity reaches 93.61%. The specific results are listed in Table 1.
[0058] Example 2
[0059] An ultra-thin core-shell structure photocatalyst and a preparation method thereof, the catalyst preparation method comprising the following steps:
[0060] Step 1: Add 40 mL of EG into a 100 mL round-bottom single-necked flask, stir and heat in a 150 °C oil bath for 30 min;
[0061] Step 2: The specific process is the same as step 2 of Example 1, and the prepared reagent solutions all use EG as the solvent;
[0062] Step 3: The specific process is the same as step 3 of Example 1;
[0063] Step 4: The specific process is the same as step 4 of Example 1;
[0064] Step 5: The specific process is the same as step 5 of Example 1;
[0065] Step 6: The specific process is the same as step 6 of Example 1.
[0066] The catalyst prepared by HAADF-STEM and EDX observations consists of Ag nanocubes with a side length of 48 nm and an Au shell with a thickness of 1.3 nm. The Au / Ag mass ratio is 1.4% as determined by inductively coupled plasma mass spectrometry. Its light absorption is mainly concentrated in 448 nm to 800 nm as determined by UV-visible diffuse reflectance spectroscopy, and the light absorption intensity is half of that of the catalyst obtained in Example 1. The photocurrent intensity of the obtained catalyst is 1.2 times that of pure Ag nanoparticles, and the Nyquist circle radius is reduced by 1.5 times.
[0067] The ultrathin core-shell structure photocatalyst prepared in Example 2 was applied to photocatalytic carbon dioxide reduction to produce methane. The specific process was the same as that of Example 1. The ultrathin core-shell structure photocatalyst was applied to photocatalytic carbon dioxide reduction to produce methane. The results are listed in Table 1.
[0068] Example 3
[0069] An ultra-thin core-shell structure photocatalyst and a preparation method thereof, the catalyst preparation method comprising the following steps:
[0070] Step 1: The specific process is the same as step 1 of Example 1;
[0071] Step 2: First, add 0.5 mL of NaSH solution with a molar concentration of 6 mM, then add 4 mL of HCl solution with a molar concentration of 3 mM after 4 minutes, then add 10 mL of PVP solution with a mass concentration of 20 mg / mL after an interval of 4 minutes, and finally add 3 mL of CF3COOAg solution with a molar concentration of 280 mM;
[0072] Step 3: The specific process is the same as step 3 of Example 1;
[0073] Step 4: The specific process is the same as step 4 of Example 1;
[0074] Step 5: The specific process is the same as step 5 of Example 1;
[0075] Step 6: The specific process is the same as step 6 of Example 1.
[0076] The catalyst prepared by HAADF-STEM and EDX observations consists of Ag nanocubes with a side length of 35 nm and an Au shell with a thickness of 1.4 nm. The Au / Ag mass ratio is 1.5% as determined by inductively coupled plasma mass spectrometry. Its light absorption is mainly concentrated in the range of 427 nm to 800 nm as determined by UV-visible diffuse reflectance spectroscopy, and the light absorption intensity is similar to that of the catalyst obtained in Example 1. The photocurrent intensity of the obtained catalyst is 1.8 times that of pure Ag nanoparticles, and the Nyquist circle radius is reduced by 8 times.
[0077] The ultrathin core-shell structure photocatalyst prepared in Example 3 was applied to photocatalytic carbon dioxide reduction to produce methane. The specific process was the same as that of Example 1. The ultrathin core-shell structure photocatalyst was applied to photocatalytic carbon dioxide reduction to produce methane. The results are listed in Table 1.
[0078] Example 4
[0079] An ultra-thin core-shell structure photocatalyst and a preparation method thereof, the catalyst preparation method comprising the following steps:
[0080] Step 1: The specific process is the same as step 1 of Example 1;
[0081] Step 2: First, add 0.5 mL of 3 mM NaSH solution, then add 4 mL of 3 mM HCl solution 4 min later, then add 10 mL of 40 mg / mL PVP solution after an interval of 4 min, and finally add 3 mL of 280 mM CF3COOAg solution;
[0082] Step 3: The specific process is the same as step 3 of Example 1;
[0083] Step 4: The specific process is the same as step 4 of Example 1;
[0084] Step 5: The specific process is the same as step 5 of Example 1;
[0085] Step 6: The specific process is the same as step 6 of Example 1.
[0086] The catalyst prepared by HAADF-STEM and EDX observations consists of Ag nano-truncated octahedrons with a side length of 30 nm and an Au shell with a thickness of 1.5 nm. The Au / Ag mass ratio is 1.7% as determined by inductively coupled plasma mass spectrometry. Its light absorption is mainly concentrated in the range of 420 nm to 800 nm as determined by UV-visible diffuse reflectance spectroscopy, and the light absorption intensity is similar to that of the catalyst obtained in Example 1. The photocurrent intensity of the obtained catalyst is 1.6 times that of pure Ag nanoparticles, and the Nyquist circle radius is reduced by 6.5 times.
[0087] The ultrathin core-shell structure photocatalyst prepared in Example 4 was applied to photocatalytic carbon dioxide reduction to produce methane. The specific process was the same as that of Example 1. The ultrathin core-shell structure photocatalyst was applied to photocatalytic carbon dioxide reduction to produce methane. The results are listed in Table 1.
[0088] Example 5
[0089] An ultra-thin core-shell structure photocatalyst and a preparation method thereof, the catalyst preparation method comprising the following steps:
[0090] Step 1: The specific process is the same as step 1 of Example 1;
[0091] Step 2: The specific process is the same as step 2 of Example 1;
[0092] Step 3: The solution from step 2 was stirred and heated in an oil bath at 150°C for 30 min. During the entire process, except for the addition of reagents, the flask was sealed with a glass stopper;
[0093] Step 4: The specific process is the same as step 4 of Example 1;
[0094] Step 5: The specific process is the same as step 5 of Example 1;
[0095] Step 6: The specific process is the same as step 6 of Example 1.
[0096] The catalyst prepared by HAADF-STEM and EDX observations consists of Ag nanocubes with a side length of 18 nm and an Au shell with a thickness of 2.1 nm. The Au / Ag mass ratio is 1.7% as determined by inductively coupled plasma mass spectrometry. Its light absorption is mainly concentrated in the range of 397 nm to 800 nm as determined by UV-visible diffuse reflectance spectroscopy, and the light absorption intensity is half of that of the catalyst obtained in Example 1. The photocurrent intensity of the obtained catalyst is 1.1 times that of pure Ag nanoparticles, and the Nyquist circle radius is reduced by 2.5 times.
[0097] The ultrathin core-shell structure photocatalyst prepared in Example 5 was applied to photocatalytic carbon dioxide reduction to produce methane. The specific process was the same as that of Example 1 in which the ultrathin core-shell structure photocatalyst was applied to photocatalytic carbon dioxide reduction to produce methane. The results are listed in Table 1.
[0098] Example 6
[0099] An ultra-thin core-shell structure photocatalyst and a preparation method thereof, the catalyst preparation method comprising the following steps:
[0100] Step 1: The specific process is the same as step 1 of Example 1;
[0101] Step 2: The specific process is the same as step 2 of Example 1;
[0102] Step 3: The solution from step 2 was stirred and heated in an oil bath at 150°C for 90 min. During the entire process, except for the addition of reagents, the flask was sealed with a glass stopper.
[0103] Step 4: The specific process is the same as step 4 of Example 1;
[0104] Step 5: The specific process is the same as step 5 of Example 1;
[0105] Step 6: The specific process is the same as step 6 of Example 1.
[0106] The catalyst prepared by HAADF-STEM and EDX observations consists of Ag nanocubes with a side length of 21 nm and an Au shell with a thickness of 1.8 nm. The Au / Ag mass ratio is 1.6% as determined by inductively coupled plasma mass spectrometry. The light absorption is mainly concentrated in the range of 402 nm to 800 nm as determined by UV-visible diffuse reflectance spectroscopy, and the light absorption intensity is 0.85 times that of the catalyst obtained in Example 1. The photocurrent intensity of the obtained catalyst is 1.6 times that of pure Ag nanoparticles, and the Nyquist circle radius is reduced by 5.5 times.
[0107] The ultrathin core-shell structure photocatalyst prepared in Example 6 was applied to photocatalytic carbon dioxide reduction to produce methane. The specific process was the same as that of Example 1. The ultrathin core-shell structure photocatalyst was applied to photocatalytic carbon dioxide reduction to produce methane. The results are listed in Table 1.
[0108] Example 7
[0109] An ultra-thin core-shell structure photocatalyst and a preparation method thereof, the catalyst preparation method comprising the following steps:
[0110] Step 1: The specific process is the same as step 1 of Example 1;
[0111] Step 2: The specific process is the same as step 2 of Example 1;
[0112] Step 3: The specific process is the same as step 3 of Example 1;
[0113] Step 4: The specific process is the same as step 4 of Example 1;
[0114] Step 5: Add 2.7 mL of the aqueous solution of Ag nanocubes obtained in step 4 and 35 μL of an aqueous solution of AuCl4H with a mass concentration of 0.5 mg / mL to 100 mL of a 10% vol methanol aqueous solution and mix well;
[0115] Step 6: The specific process is the same as step 6 of Example 1.
[0116] The catalyst prepared by HAADF-STEM and EDX observations consists of Ag nanocubes with a side length of 30 nm and an Au shell with a thickness of less than 1 nm. Au is evenly distributed but does not completely cover the Ag nanocubes. The Au / Ag mass ratio is 0.45% as determined by inductively coupled plasma mass spectrometry. The light absorption is mainly concentrated in the range of 420 nm to 800 nm as determined by UV-visible diffuse reflectance spectroscopy, and the light absorption intensity is similar to that of the catalyst obtained in Example 1. The photocurrent intensity of the obtained catalyst is 1.4 times that of pure Ag nanoparticles, and the Nyquist circle radius is reduced by 5.4 times.
[0117] The ultrathin core-shell structure photocatalyst prepared in Example 7 was applied to photocatalytic carbon dioxide reduction to produce methane. The specific process was the same as that of Example 1 in which the ultrathin core-shell structure photocatalyst was applied to photocatalytic carbon dioxide reduction to produce methane. The results are listed in Table 1.
[0118] Example 8
[0119] An ultra-thin core-shell structure photocatalyst and a preparation method thereof, the catalyst preparation method comprising the following steps:
[0120] Step 1: The specific process is the same as step 1 of Example 1;
[0121] Step 2: The specific process is the same as step 2 of Example 1;
[0122] Step 3: The specific process is the same as step 3 of Example 1;
[0123] Step 4: The specific process is the same as step 4 of Example 1;
[0124] Step 5: Add 2.7 mL of the Ag nanocube aqueous solution obtained in step 4 and 432 μL of an AuCl4H aqueous solution with a mass concentration of 0.5 mg / mL to 100 mL of a 10% vol methanol aqueous solution and mix well;
[0125] Step 6: The specific process is the same as step 6 of Example 1.
[0126] The catalyst prepared by HAADF-STEM and EDX observations consists of Ag nanocubes with a side length of 30 nm and an Au shell with a thickness of 4.0 nm. The Au / Ag mass ratio is 3.80% as determined by inductively coupled plasma mass spectrometry. Its light absorption is mainly concentrated in 420 nm to 800 nm as determined by UV-visible diffuse reflectance spectroscopy, and the light absorption intensity is similar to that of the catalyst obtained in Example 1. The photocurrent intensity of the obtained catalyst is 1.1 times that of pure Ag nanoparticles, and the Nyquist circle radius is reduced by 2.5 times.
[0127] The ultrathin core-shell structure photocatalyst prepared in Example 8 was applied to photocatalytic carbon dioxide reduction to produce methane. The specific process was the same as that of Example 1 in which the ultrathin core-shell structure photocatalyst was applied to photocatalytic carbon dioxide reduction to produce methane. The results are listed in Table 1.
[0128] Example 9
[0129] An ultra-thin core-shell structure photocatalyst and a preparation method thereof, the catalyst preparation method comprising the following steps:
[0130] Step 1: The specific process is the same as step 1 of Example 1;
[0131] Step 2: The specific process is the same as step 2 of Example 1;
[0132] Step 3: The specific process is the same as step 3 of Example 1;
[0133] Step 4: The specific process is the same as step 4 of Example 1;
[0134] Step 5: The specific process is the same as step 5 of Example 1;
[0135] Step 6: The solution in step 5 was continuously stirred and irradiated under a 300 W xenon lamp for 1.5 h. After washing the sample three times with ultrapure water, an Ag@Au photocatalyst with an ultrathin core-shell structure was obtained.
[0136] The catalyst prepared by HAADF-STEM and EDX observations consists of Ag nanocubes with a side length of 30 nm and an Au shell with a thickness of 1.0 nm. The Au / Ag mass ratio is 1.0% as determined by inductively coupled plasma mass spectrometry. Its light absorption is mainly concentrated in 420 nm to 800 nm as determined by UV-visible diffuse reflectance spectroscopy, and the light absorption intensity is similar to that of the catalyst obtained in Example 1. The photocurrent intensity of the obtained catalyst is 1.7 times that of pure Ag nanoparticles, and the Nyquist circle radius is reduced by 7.5 times.
[0137] The ultrathin core-shell structure photocatalyst prepared in Example 9 was applied to photocatalytic carbon dioxide reduction to produce methane. The specific process was the same as that of Example 1. The ultrathin core-shell structure photocatalyst was applied to photocatalytic carbon dioxide reduction to produce methane. The results are listed in Table 1.
[0138] Table 1 Photocatalytic carbon dioxide reduction performance test results
[0139]
[0140]
[0141] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An ultra-thin core-shell structure photocatalyst, characterized in that: The photocatalyst is a mixed bimetallic plasmon nanostructure material, which is composed of Ag nanocubes with a side length of 18nm to 48nm and an Au shell with an average thickness of 1nm to 4nm.
2. The ultra-thin core-shell structure photocatalyst according to claim 1, characterized in that: The Ag / Au mass ratio of the photocatalyst is 0.45% to 3.80%.
3. The ultra-thin core-shell structure photocatalyst according to claim 2, characterized in that: The photocatalyst is a mixed bimetallic plasmon nanostructure material, which is composed of Ag nanocubes with a side length of 30nm and an Au shell with an average thickness of 1.5nm. The Ag / Au mass ratio of the photocatalyst is 1.6%.
4. The method for preparing the ultra-thin core-shell structure photocatalyst according to any one of claims 1 to 3, characterized in that: The method for preparing the photocatalyst comprises the following steps: Step 1: Add 40 mL of DEG or EG into a 100 mL round-bottom single-necked flask, stir and heat in a 150 °C oil bath for 30 min; Step 2: First, add 0.5 mL of NaSH solution with a molar concentration of 3 mM to 6 mM, then add 4 mL of HCl solution with a molar concentration of 3 mM after 4 minutes, then add 10 mL of PVP solution with a mass concentration of 20 mg / mL to 40 mg / mL after an interval of 4 minutes, and finally add 3 mL of CF3COOAg solution with a molar concentration of 280 mM. The prepared reagent solutions all use DEG or EG as solvent; Step 3: Stir and heat the solution from step 2 in a 150°C oil bath for 30 to 480 min. During the entire process, except for adding reagents, the flask was sealed with a glass stopper; Step 4: After the reaction is completed, the flask is immediately placed in an ice water bath for cooling and quenching, and then washed with acetone for precipitation and then washed with ultrapure water three times to obtain Ag nanocubes, which are then dispersed in ultrapure water and prepared into a 1.855 mg / mL Ag nanocube aqueous solution; Step 5: Add 2.7 mL of the aqueous solution of Ag nanocubes obtained in step 4 and 35 μL to 432 μL of an aqueous solution of AuCl4H with a concentration of 0.5 mg / mL to 100 mL of a 10% vol methanol aqueous solution, and mix well; Step 6: The solution in step 5 was continuously stirred and irradiated for 1.5 h to 3 h under a 300 W xenon lamp for photodeposition. After washing the sample three times with ultrapure water, an ultrathin core-shell structure photocatalyst was obtained.
5. The method for preparing the ultrathin core-shell structure photocatalyst according to claim 4, characterized in that: The solvent in step 1 is DEG, and the molar concentration of the NaSH solution in step 2 is 3 mM.
6. The method for preparing the ultrathin core-shell structure photocatalyst according to claim 4, characterized in that: The mass concentration of the PVP solution in step 2 is 20 mg / mL.
7. The method for preparing the ultrathin core-shell structure photocatalyst according to claim 4, characterized in that: When the solvent in step 1 is DEG, the stirring and heating time in step 3 is 480 min.
8. The method for preparing the ultrathin core-shell structure photocatalyst according to claim 4, characterized in that: The added volume of the AuCl4H aqueous solution in step 5 is 173 μL.
9. The method for preparing the ultrathin core-shell structure photocatalyst according to claim 4, characterized in that: The photodeposition time in step six is 3 hours.
10. The ultra-thin core-shell structure photocatalyst according to any one of claims 1 to 3 is applied to photocatalytic carbon dioxide reduction to produce methane, characterized in that: The following steps are involved: Step 1: Disperse 5 mg of the ultrathin core-shell structure photocatalyst prepared according to claims 1 to 3 in 6 mL of ultrapure water, disperse by ultrasonication, drop-coat on an aluminum foil substrate, and dry under vacuum at 60°C; Step 2: Add 1.5 g of sodium bicarbonate to the bottom of the quartz reactor and place the aluminum foil substrate with the photocatalyst on the bracket; Step 3: Connect and fix the quartz reactor to the all-glass automatic online trace gas analysis system, turn on the vacuum pump and plunger pump, evacuate the reaction device, inject high-purity argon gas into the quartz reactor to evacuate again, and repeat three times; Step 4: Inject 10 mL of 0.8 M sulfuric acid into the bottom of the reactor to generate the carbon dioxide and water vapor required for the reaction, turn on the xenon lamp to react, and take samples every 20 minutes to measure the activity.