High-strength anti-cracking waterproof roll as well as preparation method and application thereof
A high-strength crack-resistant waterproof membrane with modified asphalt and nano silicon components addresses the issue of low strength and leakage in existing membranes, providing enhanced durability and water resistance.
Patent Information
- Application Number
- CN202411072426.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing modified asphalt waterproofing membranes have low membrane strength and are prone to leakage due to poor crack resistance, which affects their durability and water resistance.
A high-strength crack-resistant waterproof membrane is developed, comprising an isolation layer, support layer, and modified asphalt layer with specific raw materials like modified hydrogenated styrene-butadiene block copolymer and nano silicon, enhancing flexibility, bonding, and crack-filling capabilities.
The membrane exhibits improved flexibility, durability, and water resistance, with enhanced bonding and crack-filling properties, ensuring effective waterproofing under complex conditions.
Smart Images

Figure BDA0004981246970000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building heat-proof materials, and in particular to a high-strength crack-resistant waterproof coiled material and a preparation method and application thereof. Background Art
[0002] With the progress of various engineering constructions, water seepage and leakage problems will occur on roofs, floors, and basements. Therefore, waterproofing projects have emerged. Various waterproof materials have emerged one after another. Waterproofing membranes are widely used in the construction industry and are one of the important building materials. Modified asphalt waterproofing membranes have good waterproofing effects and are commonly used materials in waterproofing systems. However, existing modified asphalt waterproofing membranes have low membrane strength and a risk of leakage.
[0003] Therefore, there is an urgent need for a high-strength crack-resistant waterproof membrane. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention proposes a high-strength crack-resistant waterproof roll material, which is conducive to large-area paving, so that the roll material can be better bonded to the local simple-shaped waterproof base layer to ensure the effectiveness of the waterproof layer.
[0005] The present invention also provides a method for preparing the high-strength crack-resistant waterproof coiled material.
[0006] The present invention also proposes the application of the high-strength crack-resistant waterproof membrane in the engineering field.
[0007] According to one aspect of the present invention, a high-strength crack-resistant waterproof roll material is provided, comprising an isolation layer material, a support layer material and a modified asphalt layer;
[0008] The modified asphalt layer comprises the following raw materials: asphalt matrix, modified hydrogenated styrene-butadiene block copolymer and modified nano silicon;
[0009] The raw materials for preparing the modified nano-silicon include: acrylic acid azo silane copolymer and nano-silicon dioxide.
[0010] According to the embodiments of the first aspect of the present invention, there are at least the following beneficial effects:
[0011] The modified hydrogenated styrene-butadiene block copolymer is a triblock copolymer composed of styrene, ethylene and butadiene. In its structure, the combination of styrene monomer and butadiene monomer forms a hard block, while the ethylene monomer provides a soft middle block. The hydrogenated styrene-butadiene block copolymer itself has excellent elasticity and flexibility, as well as thermoplasticity and processability, which enables this component to effectively improve flexibility and durability in modified asphalt. The methyl side chain introduced by methyl methacrylate can enhance the cohesion and bonding properties of the polymer, and improve its compatibility and bonding strength with asphalt matrices.
[0012] As a reinforcing agent, nano silicon can combine with polymer chains in asphalt to significantly improve the bonding performance of asphalt coils. Filling micro cracks and pores in asphalt effectively prevents crack expansion, improves the anti-cracking ability of coils, and makes them more durable under complex road conditions. Nano silicon has some polar groups on its surface, such as hydroxyl (-OH), which make nano silicon highly hydrophilic in aqueous or polar media. Acrylic azosilane copolymer introduces hydrophobic organic chain groups, which weakens the overall hydrophilicity of nano silicon. In the asphalt matrix, the enhanced hydrophobicity of the nano silicon surface reduces its interaction with hydrophilic substances in asphalt, thereby reducing agglomeration. Functional groups such as polycarboxyl (-COOH) in asphalt form hydrogen bond interactions with acrylic acid groups, effectively combining with polymer chains in asphalt, can fill micro gaps and cracks in the asphalt matrix to form a stronger interface bond, so that the modified nano silicon forms a continuous heat conduction channel, improves the high temperature stability and heat resistance of asphalt, reduces softening and deformation caused by high temperature, and improves water resistance.
[0013] In some embodiments of the present invention, the method for preparing the modified hydrogenated styrene-butadiene block copolymer comprises: mixing and reacting the hydrogenated styrene-butadiene block copolymer, methyl methacrylate, a surfactant, and a crosslinking agent.
[0014] In some embodiments of the present invention, the surfactant comprises a nonionic surfactant.
[0015] In some embodiments of the present invention, the nonionic surfactant comprises sodium dodecylbenzene sulfonate.
[0016] In some embodiments of the invention, the cross-linking agent comprises dimethylacrylamide.
[0017] The MMA monomer combines with the SEBS polymer through polymerization reaction, and the introduced crosslinking agent DMAA can form crosslinking points with the SEBS polymer during the reaction, enhancing the structural stability and mechanical properties of the polymer. The surfactant improves the interfacial compatibility between the modified polymer and asphalt, allowing the modified polymer to be better dispersed in the asphalt, thereby improving the bonding performance and cohesion of the asphalt.
[0018] In some embodiments of the present invention, the raw material for preparing the isolation layer includes: at least one of a PE film and a PET film.
[0019] In some embodiments of the present invention, the raw materials for preparing the support layer include: glass fiber reinforced polyester tire.
[0020] In some embodiments of the present invention, the raw materials for preparing the high-strength crack-resistant waterproof membrane further include: engine oil.
[0021] In some embodiments of the present invention, the raw materials for preparing the modified asphalt layer include, by weight: 55-65 parts of asphalt matrix, 15-18 parts of hydrogenated styrene-butadiene block copolymer and 0.3-0.5 parts of modified nano-silicon.
[0022] According to two aspects of the present invention, a method for preparing a high-strength crack-resistant waterproof roll material is proposed, comprising: forming an upper modified asphalt layer and a lower modified asphalt layer on the upper and lower surfaces of a support layer, respectively, covering the upper modified asphalt layer and the lower modified asphalt layer with an upper surface isolation layer and a lower surface isolation layer, respectively, and then cooling.
[0023] In some embodiments of the present invention, the method for preparing the modified asphalt layer comprises: heating an asphalt matrix and then heating and mixing the asphalt matrix with modified nano-silicon and hydrogenated styrene-butadiene block copolymer.
[0024] In some embodiments of the present invention, the method for preparing the modified nano-silicon comprises: dispersing nano-silicon dioxide and acrylic acid azosilane copolymer and then mixing them for reaction.
[0025] In some embodiments of the present invention, the method for preparing the acrylic acid azosilane copolymer comprises:
[0026] A1. Dissolve trimethoxysilylpropyltrichlorosilane in chloroform and add acrylic acid at 0-5°C for 2-4 hours to obtain a precursor of a silane coupling agent;
[0027] A2. React the precursor of the silane coupling agent and hydrochloric acid at 20-30° C. for 12-24 hours to obtain an acrylic acid azosilane copolymer.
[0028] In some embodiments of the present invention, the temperature at which the asphalt matrix is heated is 140-150°C.
[0029] According to three aspects of the present invention, a high-strength crack-resistant waterproof membrane for use in the engineering field is proposed. DETAILED DESCRIPTION
[0030] The words "preferably", "more preferably", etc. in the present invention refer to embodiments of the present invention that may provide certain beneficial effects in certain circumstances. However, other embodiments may also be preferred under the same circumstances or other circumstances. In addition, the description of one or more preferred embodiments does not imply that other embodiments are not applicable, nor is it intended to exclude other embodiments from the scope of the present invention.
[0031] When a numerical range is disclosed herein, the above range is considered to be continuous and includes the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0032] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of the present invention.
[0033] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0034] Example 1
[0035] This embodiment prepares a high-strength crack-resistant waterproof membrane, which is as follows:
[0036] The modified asphalt layer material is pumped into the dipping tank at the front end of the production line, and an upper modified asphalt layer and a lower modified asphalt layer are formed on the upper and lower surfaces of the glass fiber reinforced polyester tire through pre-impregnation and squeezing processes respectively. The upper modified asphalt layer and the lower modified asphalt layer are respectively covered with PE film to form an upper surface isolation layer and a lower surface isolation layer. After cooling by cooling equipment, the finished products are measured, trimmed, rolled and packaged.
[0037] The preparation method of the modified asphalt layer is:
[0038] Add 55 kg of 90# petroleum asphalt and engine oil into the reactor, heat to 140°C, stir at low speed for 30 minutes, then add 0.3 kg of modified nano-silicon, stir at 1000 r / min for 1 hour, raise the temperature of the reactor to 175°C, add 15 kg of modified hydrogenated styrene-butadiene block copolymer, continue stirring and mixing for 1.5 hours, and finally shear at 1000 r / min for 90 minutes to obtain the modified asphalt layer material.
[0039] The preparation method of modified nano silicon is:
[0040] A1. 10 g of trimethoxysilylpropyltrichlorosilane was added to 50 mL of chloroform and fully dissolved, and then 3 g of acrylic acid was added at 0 ° C. The reaction time was 2 hours;
[0041] A2. React the precursor of the silane coupling agent and hydrochloric acid at a pH between 2 and 4 at 20 to 30° C. for 12 to 24 hours to obtain an acrylic acid azosilane copolymer.
[0042] A3. Add 10 g of nano-silica to about 200 mL of chloroform, and then add 1 g of acrylic acid azosilane copolymer after ultrasonic treatment or mechanical stirring. React at 20°C for 12 h to obtain modified nano-silica.
[0043] Example 2
[0044] This embodiment prepares a high-strength crack-resistant waterproof membrane. The difference between this embodiment and embodiment 2 is that the asphalt matrix is 65 parts, the hydrogenated styrene-butadiene block copolymer is 18 parts and the modified nano-silicon is 0.5 parts, and the other conditions are the same.
[0045] Example 3
[0046] This embodiment prepares a high-strength crack-resistant waterproof membrane. The difference between this embodiment and embodiment 2 is that the asphalt matrix is 60 parts, the hydrogenated styrene-butadiene block copolymer is 16 parts and the modified nano-silicon is 0.4 parts, and the other conditions are the same.
[0047] Comparative Example 1
[0048] This comparative example prepares a high-strength crack-resistant waterproof coiled material, which differs from Example 1 in that unmodified nano-silicon is used, and the other conditions are the same as those of Example 1.
[0049] Comparative Example 2
[0050] This comparative example prepares a high-strength crack-resistant waterproof membrane, which differs from Example 1 in that an unmodified hydrogenated styrene-butadiene block copolymer is used, and the other conditions are the same as those of Example 1.
[0051] Comparative Example 2
[0052] This comparative example prepares an airport pavement concrete surface treatment agent with enhanced wear resistance. The only difference from Example 5 is that unmodified hydrogenated styrene-butadiene block copolymer is added, and the other conditions are the same as Example 1.
[0053] Test example
[0054] This test example tests the performance of the high-strength crack-resistant waterproof membrane prepared in Example 1 and Comparative Example 1. The results are shown in Table 1:
[0055] The impermeability of high-strength self-adhesive waterproof materials was tested according to the experimental method of standard JC / T684-1997;
[0056] Conduct mechanical property tests according to the national standard GB18242-2008 "Elastomer modified asphalt waterproofing membrane";
[0057] Table 1 Performance of concrete surface treatment agent
[0058]
[0059] The results are shown in Table 1. From the examples and comparative example 1 in Table 1, it can be seen that the hydrogenated styrene-butadiene block copolymer has compatibility problems with the asphalt substrate, resulting in poor stability and enhancement effect in the asphalt. The copolymer may react, resulting in a gradual decline in its performance, affecting the service life and water resistance of the coiled material. From the examples and comparative example 2 in Table 1, it can be seen that the unmodified nano silicon particles are easily agglomerated in the asphalt, which will cause the uniform dispersion of the nano silicon in the asphalt to deteriorate, making it impossible for the nano silicon to effectively fill the microscopic voids and cracks of the asphalt, resulting in a decrease in the compactness and water resistance of the asphalt coiled material, thereby making the coiled material more susceptible to water intrusion, thereby affecting its waterproof performance. At the same time, the unmodified nano silicon may not be able to effectively combine with the polymer chain in the asphalt, and cannot effectively improve the mechanical properties of the asphalt coiled material, such as tensile strength and durability. In the modified hydrogenated styrene-butadiene block copolymer in the embodiment, the triblock copolymer composed of styrene, ethylene and butadiene is formed, and the combination of styrene monomer and butadiene monomer in its structure forms a hard block, while the ethylene monomer provides a soft middle block. It has thermoplasticity and processability at the same time, so that this component can effectively improve the flexibility and durability in modified asphalt. Nanosilicon acts as a reinforcing agent to fill the micro cracks and pores in the asphalt. It can fill the micro voids and cracks in the asphalt matrix to form a stronger interface bond, so that the modified nanosilicon forms a continuous heat conduction channel, improves the high-temperature stability and heat resistance of the asphalt, reduces the softening and deformation caused by high temperature, and improves the water resistance.
[0060] The above content describes the embodiments of the present invention in detail, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
Claims
1. A high-strength crack-resistant waterproof membrane, It is characterized in that It includes isolation layer material, support layer material and modified asphalt layer; The modified asphalt layer comprises the following raw materials: asphalt matrix, modified hydrogenated styrene-butadiene block copolymer and modified nano-silicon; The raw materials for preparing the modified nano-silicon include: acrylic acid azo silane copolymer and nano-silicon dioxide; The raw materials for preparing the modified hydrogenated styrene-butadiene block copolymer include: hydrogenated styrene-butadiene block copolymer and methyl methacrylate.
2. The high-strength crack-resistant waterproof membrane according to claim 1, It is characterized in that The raw material for preparing the isolation layer includes at least one of a PE film and a PET film.
3. The high-strength crack-resistant waterproof membrane according to claim 1, It is characterized in that The raw materials for preparing the support layer include: glass fiber reinforced polyester tire.
4. The high-strength crack-resistant waterproof membrane according to claim 1, It is characterized in that The raw materials for preparing the high-strength anti-cracking waterproof coiled material also include: engine oil.
5. The high-strength crack-resistant waterproof membrane according to claim 1, It is characterized in that The raw materials for preparing the modified asphalt layer include, by weight: 55-65 parts of asphalt matrix, 15-18 parts of hydrogenated styrene-butadiene block copolymer and 0.3-0.5 parts of modified nano silicon.
6. The method for preparing the high-strength crack-resistant waterproof membrane according to any one of claims 1 to 5, It is characterized in that include: An upper modified asphalt layer and a lower modified asphalt layer are formed on the upper and lower surfaces of the support layer respectively, and an upper surface isolation layer and a lower surface isolation layer are respectively covered on the upper modified asphalt layer and the lower modified asphalt layer and then cooled.
7. The method for preparing the high-strength crack-resistant waterproof coiled material according to claim 6, It is characterized in that The preparation method of the modified asphalt layer comprises: heating an asphalt matrix and then heating and mixing the asphalt matrix with modified nano silicon and hydrogenated styrene-butadiene block copolymer.
8. The method for preparing the high-strength crack-resistant waterproof coiled material according to claim 7, It is characterized in that The preparation method of the modified nano silicon comprises: dispersing nano silicon dioxide and acrylic acid azo silane copolymer and then mixing them for reaction.
9. The method for preparing the high-strength crack-resistant waterproof coiled material according to claim 7, It is characterized in that The temperature at which the asphalt matrix is heated is 140-150°C.
10. Use of the high-strength crack-resistant waterproof membrane according to any one of claims 1 to 9 in the engineering field.