Cellulose aerogel and preparation method thereof
By preparing cellulose aerogels with high transparency, low haze and strong thermal insulation, the problem of limited application of existing silica aerogels in buildings is solved, and an efficient and low-cost building energy-saving material is provided. .
Patent Information
- Application Number
- CN202411329763.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-12-03
AI Technical Summary
The existing application of silica aerogels in construction is limited by their brittleness, poor mechanical properties and high cost. At the same time, few research on transparent cellulose aerogels has led to limited application in the field of building energy conservation.
By providing a method for preparing cellulose aerogel, including homogenization treatment, centrifugal treatment, formation of directional fiber system and glue formation process of TEMPO oxidized cellulose aqueous dispersion, combined with supercritical drying technology, high transparency is prepared, Cellulose aerogel with low haze and strong thermal insulation ability.
It realizes the high transparency, low haze and strong insulation capabilities of cellulose aerogels, reduces costs, and provides an alternative to silica aerogels, suitable for building energy conservation.
Smart Images

Figure CN119060402A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aerogel materials, and in particular to a cellulose aerogel and a preparation method thereof. Background Art
[0002] In the field of building energy conservation, almost 30% of energy losses are caused by windows. Transparent insulation materials can not only reduce building energy consumption, but also meet the requirements of visual interaction. Aerogel is a low-density solid material with high porosity and extremely low thermal conductivity. It has been widely used in thermal insulation in aerospace, building envelopes, and new energy vehicles. However, as the most widely used and most mature type of aerogel, silica aerogel has the disadvantages of being brittle and fragile, and having poor mechanical properties. Its cost is about 10 times higher than that of conventional materials. Therefore, it is not currently widely used in buildings.
[0003] Cellulose is the most abundant natural renewable resource on earth. As a biomass material, it has the advantages of high elasticity, low cost and green and pollution-free. The aerogel material prepared from it may become a substitute for silica aerogel in the future. At present, the research on transparent cellulose aerogel materials is not extensive. Although the use of cellulose-based materials can improve the flexibility of aerogels, due to differences in cellulose types and preparation methods, the self-assembly of cellulose chains will cause uneven nanostructure sizes. Generally, the prepared cellulose-based aerogel materials have a large pore size, which will increase the thermal conductivity of the aerogel. At the same time, the light transmittance is relatively poor, and there are also problems such as haze. For example, the Chinese patent with publication number CN107722338A discloses a method for preparing nanocellulose aerogel and nanocellulose aerogel, which oxidizes the slurry to obtain a suspension slurry; then the suspension slurry is treated to neutrality by dialysis, and then a freeze-drying protective agent is added, and a cyclic high-pressure treatment is used to obtain nanocellulose; finally, the nanocellulose is freeze-dried to obtain a nanocellulose aerogel. Although the above preparation method improves the mechanical properties and specific surface area of the nanocellulose aerogel, the obtained nanocellulose aerogel is completely white and has no transparency. Summary of the invention
[0004] In view of this, the object of the present invention is to provide a cellulose aerogel and a preparation method thereof. The cellulose aerogel obtained by the preparation method provided by the present invention has high transparency, low haze, and strong heat insulation ability.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The invention provides a method for preparing cellulose aerogel, comprising the following steps:.
[0007] Providing a TEMPO oxidized cellulose aqueous dispersion;
[0008] The TEMPO oxidized cellulose aqueous dispersion is subjected to homogenization and centrifugation in sequence to obtain a centrifugal system;
[0009] After the centrifugal system is formed into a membrane, the first hydrochloric acid solution is sprayed into the membrane, and then the membrane is allowed to stand to obtain an oriented fiber system;
[0010] The oriented fiber system is immersed in a second hydrochloric acid solution to form a gel to obtain a hydrogel;
[0011] The hydrogel is sequentially washed, solvent replaced and dried to obtain the cellulose aerogel.
[0012] Preferably, the method for preparing TEMPO oxidized cellulose in the TEMPO oxidized cellulose aqueous dispersion comprises the following steps:
[0013] After mixing cellulose, 2,2,6,6-tetramethylpiperidin-1-oxyl free radical, sodium bromide and water, sodium hypochlorite is added, and then a first oxidation is performed under alkaline conditions to obtain a pre-oxidized cellulose dispersion;
[0014] After the pre-oxidized cellulose dispersion, 2,2,6,6-tetramethylpiperidin-1-oxyl free radical and sodium chlorite are mixed, sodium hypochlorite is added, and then a second oxidation is performed under acidic conditions to obtain the TEMPO oxidized cellulose.
[0015] Preferably, during the first oxidation process, the mass ratio of the cellulose, 2,2,6,6-tetramethylpiperidin-1-oxyl free radical and sodium bromide is 20:0.1-1:1-5; the amount ratio of the cellulose and sodium hypochlorite is 1 g:1-15 mmol;
[0016] The alkaline pH value is 9 to 14;
[0017] The temperature of the first oxidation is 10 to 65°C;
[0018] After the first oxidation, dialysis is further performed to obtain the pre-TEMPO oxidized cellulose dispersion and the dialysate, respectively.
[0019] Preferably, during the second oxidation process, the mass ratio of the 2,2,6,6-tetramethylpiperidin-1-oxyl free radical, sodium chlorite and cellulose is 0.1-0.75 g:10-40:20; the dosage ratio of the sodium hypochlorite and cellulose is 10-200 mmol:20 g;
[0020] The acidic pH value is 4 to 6.8;
[0021] The temperature of the second oxidation is 10 to 65° C. and the time is 24 to 72 hours;
[0022] After the second oxidation, dialysis is further performed, and the obtained dialysis dispersion is freeze-dried to obtain the TEMPO oxidized cellulose.
[0023] Preferably, the mass concentration of the TEMPO oxidized cellulose aqueous dispersion is 0.5-3%.
[0024] Preferably, the pressure of the homogenization treatment is 50-200 MPa, the number of homogenization treatments is 1-4 times, and the time of each homogenization treatment is 10-60 min;
[0025] The rotation speed of the centrifugal treatment is 6000-8000 rpm, and the time is 10 minutes.
[0026] Preferably, the concentration of the first hydrochloric acid solution is 0.1-1 mol / L, and after the first hydrochloric acid solution is sprayed, the pH of the resulting system is ≤3;
[0027] The spraying method is atomized spray;
[0028] The standing time is 15 to 60 minutes.
[0029] Preferably, the concentration of the second hydrochloric acid solution is 0.05 to 1 mol / L, the concentration ratio of the second hydrochloric acid solution to the first hydrochloric acid solution is 1:1 to 10, and the gelling time is 4 to 24 hours.
[0030] Preferably, the drying method is supercritical drying.
[0031] The present invention also provides a cellulose aerogel prepared by the preparation method described in the above technical solution, wherein the thermal conductivity of the cellulose aerogel is 0.01-0.04 W / (m·K), the average visible light transmittance is 70-90%, and the haze is 10-90%.
[0032] The invention provides a method for preparing cellulose aerogel.
[0033] The present invention homogenizes the TEMPO oxidized cellulose aqueous dispersion, and can control the TEMPO oxidized cellulose diameter to be uniformly distributed at about 20 nm, which is conducive to preparing a uniform and stable cellulose pore structure, increasing the light transmittance of cellulose aerogel, and reducing visual haze. Then, centrifugation can remove bubbles and also improve the light transmittance of cellulose aerogel. At the same time, after the centrifugal system forms a film, the present invention sprays a first hydrochloric acid solution and then allows it to stand. After the first hydrochloric acid solution is sprayed, the TEMPO oxidized cellulose will be arranged in a directional and orderly manner. Combined with the subsequent gelation, a cellulose aerogel with high light transmittance, low haze, and strong thermal insulation can be obtained.
[0034] Furthermore, the preparation method of TEMPO oxidized cellulose in the TEMPO oxidized cellulose aqueous dispersion comprises the following steps: after mixing cellulose, 2,2,6,6-tetramethylpiperidine-1-oxyl free radical, sodium bromide and water, sodium hypochlorite is added, and then a first oxidation is performed under alkaline conditions to obtain a pre-oxidized cellulose dispersion; after mixing the pre-oxidized cellulose dispersion, 2,2,6,6-tetramethylpiperidine-1-oxyl free radical and sodium chlorite, sodium hypochlorite is added, and then a second oxidation is performed under acidic conditions to obtain the TEMPO oxidized cellulose. The TEMPO oxidized cellulose of the present invention is obtained by two-step oxidation of alkaline oxidation and acidic oxidation, so that the cellulose is oxidized more thoroughly and has a higher carboxyl content, thereby improving the dispersibility of cellulose and ultimately further improving the transparency of cellulose aerogel.
[0035] Furthermore, the spraying method is atomized spray, and the first hydrochloric acid solution is sprayed in the form of atomized spray, which can make the surface of the transparent cellulose gel smooth to the maximum extent, reduce cellulose surface scattering, increase light transmittance, and reduce haze.
[0036] Furthermore, the drying method is supercritical drying. The supercritically dried transparent cellulose aerogel has a uniform internal structure, high light transmittance and low haze, and has good thermal insulation function. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 This is a physical photo of the cellulose aerogel obtained in Example 1. DETAILED DESCRIPTION
[0038] The present invention provides a method for preparing cellulose aerogel, comprising the following steps:
[0039] Providing a TEMPO oxidized cellulose aqueous dispersion;
[0040] The TEMPO oxidized cellulose aqueous dispersion is subjected to homogenization and centrifugation in sequence to obtain a centrifugal system;
[0041] After the centrifugal system is formed into a membrane, the first hydrochloric acid solution is sprayed into the membrane, and then the membrane is allowed to stand to obtain an oriented fiber system;
[0042] The oriented fiber system is immersed in a second hydrochloric acid solution to form a gel to obtain a hydrogel;
[0043] The hydrogel is sequentially washed, solvent replaced and dried to obtain the cellulose aerogel.
[0044] In the present invention, unless otherwise specified, the raw materials used in the present invention are preferably commercially available products.
[0045] The present invention provides a TEMPO oxidized cellulose aqueous dispersion.
[0046] In the present invention, the mass concentration of the TEMPO oxidized cellulose aqueous dispersion is preferably 0.5-3%, specifically 0.5%, 1%, 1.5%, 2%, 2.5% or 3%. In the present invention, the TEMPO oxidized cellulose aqueous dispersion is preferably frozen for future use.
[0047] In the present invention, the method for preparing TEMPO oxidized cellulose in the TEMPO oxidized cellulose aqueous dispersion preferably comprises the following steps:
[0048] After mixing cellulose, 2,2,6,6-tetramethylpiperidin-1-oxyl free radical, sodium bromide and water, sodium hypochlorite is added, and then a first oxidation is performed under alkaline conditions to obtain a pre-oxidized cellulose dispersion;
[0049] After the pre-oxidized cellulose dispersion, 2,2,6,6-tetramethylpiperidin-1-oxyl free radical and sodium chlorite are mixed, sodium hypochlorite is added, and then a second oxidation is performed under acidic conditions to obtain the TEMPO oxidized cellulose.
[0050] The invention mixes cellulose, 2,2,6,6-tetramethylpiperidin-1-oxyl free radical, sodium bromide and water, then adds sodium hypochlorite, and then performs first oxidation under alkaline conditions to obtain a pre-oxidized cellulose dispersion. In the present invention, during the first oxidation process, the mass ratio of the cellulose, 2,2,6,6-tetramethylpiperidin-1-oxyl free radical and sodium bromide is preferably 20:0.1-1:1-5, more preferably 20:0.3-0.6:2-4, specifically 20:0.32:2, 20:0.1:1, 20:0.1:5, 20:1:1, 20:1:5, 20:0.3:1, 20:0.3:5, 20:0.5:1, 20:0.5:5, 20:0.1:2, 20:0.1:3, 20:0.1:4 or 20:0.1:5; the dosage ratio of the cellulose and sodium hypochlorite is preferably 1 g:1-15 mmol, specifically 1 g:1 mmol, 1 g:5 mmol, 1 g:10 mmol or 1 g:15 mmol. In the present invention, the temperature of mixing cellulose, 2,2,6,6-tetramethylpiperidin-1-oxyl radical, sodium bromide and water is preferably room temperature, and the mixing of cellulose, 2,2,6,6-tetramethylpiperidin-1-oxyl radical, sodium bromide and water is preferably carried out under stirring, and the stirring time is preferably 6 to 14 hours. In the present invention, the alkaline pH value is preferably 9 to 14, specifically 9, 10, 11, 12, 13 or 14, and the alkaline regulating agent is preferably a sodium hydroxide aqueous solution, and the mass concentration of the sodium hydroxide aqueous solution is preferably 0.5 mol / L. In the present invention, the temperature of the first oxidation is preferably 10 to 65°C, more preferably 10 to 35°C, specifically 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C or 65°C; the present invention does not specifically limit the time of the first oxidation, as long as the pH value of the system no longer decreases, the first oxidation reaction can be considered to be completed and the subsequent operation can be directly carried out.
[0051] After the first oxidation, the present invention preferably further comprises dialysis to obtain the pre-TEMPO oxidized cellulose dispersion and the dialysate, respectively. In the present invention, the dialysis time is preferably 7 days, and during the dialysis process, the deionized water is preferably replaced every 24 hours.
[0052] After obtaining the pre-oxidized cellulose dispersion, the present invention mixes the pre-oxidized cellulose dispersion, 2,2,6,6-tetramethylpiperidin-1-oxyl free radical and sodium chlorite, then adds sodium hypochlorite, and then performs a second oxidation under acidic conditions to obtain the TEMPO oxidized cellulose.
[0053] In the present invention, during the second oxidation process, the mass ratio of the 2,2,6,6-tetramethylpiperidine-1-oxyl free radical, sodium chlorite and cellulose is preferably 0.1-0.75:10-40:20, more preferably 0.3-0.6:20-30:20, specifically 0.5:22.6:20; the dosage ratio of sodium hypochlorite and cellulose is preferably 10-200mmol:20g, more preferably 100-150mmol:20g, specifically 10mmol:20g, 50mmol:20g, 100mmol:20g, 136mmol:20g, 150mmol:20g or 200mmol:20g. In the present invention, the sodium hypochlorite is preferably used in the form of a sodium hypochlorite solution, and the concentration of the sodium hypochlorite solution is preferably 1.36 mol / L; the solvent of the sodium hypochlorite solution is preferably a buffer solution, and the preparation method of the buffer solution preferably comprises the following steps: adjusting the pH of the dialysate to 4.8-6.8 to obtain an acidic dialysate; adding 47 mL of a 1 mol / L dibasic sodium phosphate solution and 53 mL of a 1 mol / L monobasic sodium phosphate solution to 2 L of the acidic dialysate, and stirring at 500 rpm for 5 min to obtain the buffer solution.
[0054] In the present invention, the mixing of the pre-oxidized cellulose dispersion, 2,2,6,6-tetramethylpiperidin-1-oxyl free radical and sodium chlorite is preferably carried out under stirring, and the stirring speed is preferably 500rpm, and the time is preferably 20min. After the sodium hypochlorite is added, the present invention preferably seals the reaction container and stirs at 500rpm for 30min. In the present invention, the acidic pH value is preferably 4.8-6.8. In the present invention, the temperature of the second oxidation is preferably 10-65°C, more preferably 40-60°C, and the time is preferably 24-72h; the second oxidation is preferably carried out under water bath conditions. After the second oxidation, the present invention preferably further includes dialysis, and the obtained dialysis dispersion is freeze-dried to obtain the TEMPO oxidized cellulose. In the present invention, the dialysis time is preferably 7 days, and during the dialysis process, the deionized water is preferably replaced every 24h. In the present invention, the freeze-drying parameters preferably include: the freezing time is preferably 12h, and the drying time is preferably 72h.
[0055] The present invention subjects cellulose to alkaline oxidation and acidic oxidation, so that the cellulose is oxidized more thoroughly and has a higher carboxyl content, thereby improving the dispersibility of TEMPO oxidized cellulose and ultimately further improving the transparency of cellulose aerogel.
[0056] After providing the TEMPO oxidized cellulose aqueous dispersion, the present invention sequentially performs homogenization and centrifugation on the TEMPO oxidized cellulose aqueous dispersion to obtain a centrifugal system.
[0057] In the present invention, the pressure of the homogenization treatment is preferably 50 to 200 MPa, more preferably 100 to 150 MPa, specifically 50 MPa, 100 MPa, 150 MPa or 200 MPa; the number of homogenization treatments is preferably 1 to 4 times, and the time for each homogenization treatment is preferably 10 to 60 min, more preferably 20 to 50 min, and more preferably 30 to 40 min.
[0058] In the present invention, the homogenization treatment can control the diameter of TEMPO oxidized cellulose to be uniformly distributed at about 20 nm, which is beneficial to prepare a uniform and stable cellulose pore structure, increase the light transmittance of cellulose aerogel, and reduce visual haze.
[0059] In the present invention, the rotation speed of the centrifugal treatment is preferably 6000-8000 rpm, specifically 6000 rpm, 6500 rpm, 7000 rpm, 7500 rpm, 7800 rpm or 8000 rpm; and the time is preferably 10 min.
[0060] In the present invention, the particle size of cellulose in the centrifugal system is preferably 10 to 40 nm in diameter.
[0061] In the present invention, the centrifugation can remove bubbles. The cellulose particles after homogenization are small in size and are in a cellulose suspension. Even if centrifuged, no precipitation will occur and the cellulose suspension is in a uniformly distributed state. The centrifugation is only to remove bubbles to improve the transmittance of the final cellulose aerogel.
[0062] After the centrifugal system is obtained, the present invention forms a membrane of the centrifugal system, sprays the first hydrochloric acid solution into the membrane, and then allows the membrane to stand to obtain an oriented fiber system.
[0063] In the present invention, the thickness of the film is preferably 3 to 6 mm, specifically 3 mm, 4 mm, 5 mm or 6 mm; the film formation is preferably carried out in a mold.
[0064] In the present invention, the concentration of the first hydrochloric acid solution is preferably 0.1-1 mol / L, specifically 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L or 1 mol / L. In the present invention, after the first hydrochloric acid solution is sprayed, the pH of the resulting system is preferably ≤3. In the present invention, the spraying method is preferably atomized spray. In the present invention, the standing time is preferably 30 min.
[0065] The present invention controls the injection of the first hydrochloric acid solution so that the pH of the centrifugal system is ≤3. At this time, the TEMPO oxidized cellulose in the centrifugal system will be oriented and orderly arranged, and combined with the subsequent gelation, a cellulose aerogel with high light transmittance and low haze can be obtained. Furthermore, the first hydrochloric acid solution is sprayed in the form of atomization, which can make the surface of the transparent cellulose gel smooth to the maximum extent, reduce cellulose surface scattering, increase light transmittance, and reduce haze.
[0066] After obtaining the oriented fiber system, the present invention immerses the oriented fiber system in a second hydrochloric acid solution to form gel to obtain a hydrogel.
[0067] In the present invention, the concentration of the second hydrochloric acid solution is preferably 0.05-1 mol / L, specifically 0.05 mol / L, 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L or 1 mol / L; the concentration ratio of the second hydrochloric acid solution to the first hydrochloric acid solution is preferably 1:1-10, more preferably 1:4-6, specifically 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9 or 1:10; the gelling time is preferably 4-24 h.
[0068] In the present invention, during the gelation process, the cellulose arranged in an orderly and directional manner can form a uniform nanoscale cellulose gel pore structure, and the uniform nanoscale cellulose gel pore structure can ensure the light transmittance and haze of the cellulose aerogel.
[0069] After obtaining the hydrogel, the present invention sequentially washes, replaces the solvent and dries the hydrogel to obtain the cellulose aerogel.
[0070] In the present invention, the washing agent is preferably deionized water. The present invention does not specifically limit the number of washings and the amount of the washing agent, as long as the pH value of the washing solution is neutral.
[0071] In the present invention, the solvent replacement preferably includes: immersing the washed hydrogel in an ethanol aqueous solution, performing a first exchange, immersing it in ethanol, performing a second exchange, and obtaining an ethanol gel. In the present invention, the volume concentration of the ethanol aqueous solution is preferably 50%, the temperature of the first exchange is preferably 20 to 50°C, and the time is preferably 6 to 24 hours. In the present invention, the temperature of the second exchange is preferably 20 to 50°C, the number of the second exchange is preferably 2 to 8 times, and the time of each exchange is preferably 6 to 24 hours.
[0072] In the present invention, the drying method is preferably supercritical drying. In the present invention, the supercritical drying preferably includes a carbon dioxide intake stage, a carbon dioxide extraction stage and a carbon dioxide exhaust stage in sequence; the parameters of the carbon dioxide intake stage include: the temperature is preferably 5°C, the flow rate of carbon dioxide is preferably 1-2nL / min, and the holding time is preferably 3-8h. In the present invention, the parameters of the carbon dioxide extraction stage include: the pressure is preferably 10MPa, the temperature is preferably 35-50°C, and the holding time is preferably 0.5-12h. In the present invention, the parameters of the carbon dioxide exhaust stage include: the temperature is preferably 35-50°C, the flow rate of carbon dioxide is preferably 50-150mL / min, and the holding time is preferably 6-18h. In the present invention, the supercritical drying is preferably carried out in a supercritical dryer.
[0073] The present invention also provides a cellulose aerogel prepared by the preparation method described in the above technical solution, wherein the thermal conductivity of the cellulose aerogel is 0.01-0.04 W / (m·K), the average visible light transmittance is 70-90%, and the haze is 10-35%.
[0074] The cellulose aerogel and the preparation method thereof provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0075] Example 1
[0076] A method for preparing cellulose aerogel comprises the following steps:
[0077] S1. Prepare a 1% TEMPO oxidized cellulose aqueous dispersion, mix thoroughly and refrigerate in an ice bath at 5°C.
[0078] S2. Place the prepared TEMPO oxidized cellulose aqueous dispersion in a high-pressure homogenizer for homogenization. The pressure is set to 200 MPa. The homogenization times are 3 times, and each homogenization time is 30 minutes.
[0079] S3. The homogenized system was placed in a centrifuge and centrifuged at 7800 rpm for 10 min. The obtained centrifuged system was then poured into a 4 mm custom mold to form a film.
[0080] S4. Spray 0.5 mol / L hydrochloric acid solution into the membrane centrifugal system in the customized mold through an electric fogger in the form of a spray, so that the pH of the centrifugal system is less than 3, and then let it stand for 0.5 h to obtain an oriented fiber system; immerse the oriented fiber system in a 0.1 mol / L hydrochloric acid solution for 24 h to form a hydrogel.
[0081] S5. After washing away the excess acid on the surface of the hydrogel with deionized water, the hydrogel is first placed in an ethanol aqueous solution with a volume concentration of 50% for a first exchange of 12 hours at room temperature; then immersed in ethanol for a second exchange to obtain an ethanol gel, the second exchange is performed 7 times, each exchange lasts 12 hours at room temperature; then the ethanol gel is placed in a supercritical dryer for drying; wherein the drying comprises sequentially performing a carbon dioxide intake stage, a carbon dioxide extraction stage and a carbon dioxide exhaust stage; the parameters of the carbon dioxide intake flushing stage include: a temperature of 5°C, a carbon dioxide flow rate of 2nL / min, and a holding time of 5h; the parameters of the carbon dioxide extraction stage include: a pressure of 10MPa, a temperature of 40°C, and a holding time of 2h; the parameters of the carbon dioxide exhaust stage include: a temperature of 40°C, a carbon dioxide flow rate of 80mL / min, and a holding time of 10h to obtain a cellulose aerogel.
[0082] The preparation method of TEMPO oxidized cellulose is as follows:
[0083] 20 g of cellulose was suspended in 2 L of water containing 0.32 g of 2,2,6,6-tetramethylpiperidin-1-oxyl free radical (TEMPO) and sodium bromide (2 g), and stirred continuously at room temperature. NaClO (10 mmol per gram of cellulose) was added to initiate the TEMPO-mediated first oxidation for 6 h. The pH of the system was maintained at 10 by adding 0.5 mol / L NaOH solution until the pH value of the system no longer decreased and the first oxidation was completed. The obtained first oxidation liquid was then placed in a dialysis bag and dialyzed for 1 week. During this period, deionized water was replaced every 24 h to remove the reaction residual substances in the water, and a pre-TEMPO-oxidized cellulose dispersion and a dialyzate were obtained, respectively.
[0084] The pH of the dialysate was adjusted to 6 to obtain an acidic dialysate; 47 mL of 1 mol / L dibasic sodium phosphate solution and 53 mL of 1 mol / L monobasic sodium phosphate solution were added to 2 L of the acidic dialysate and stirred at 500 rpm for about 5 min to prepare a buffer solution. NaClO (136 mmol) was added to 100 mL of the buffer solution to obtain a NaClO solution.
[0085] TEMPO (0.5 g) and NaClO2 (22.6 g) were added to the pre-TEMPO oxidized cellulose dispersion and stirred at 800 rpm for 20 min until the additives were completely dissolved. Then 100 mL of NaClO solution was added and the reaction vessel was immediately sealed; the system was stirred at 500 rpm for 30 min, and then the water bath was heated to 60 ° C and the reaction was allowed to run continuously for 72 h. After the reaction was completed, the solution was placed in a dialysis bag for 1 week, during which deionized water was replaced every 24 h to remove the reaction residues in the water. The final solution was placed in a freeze dryer for 12 h and dried for 72 h to obtain TEMPO oxidized cellulose.
[0086] The thermal conductivity of the obtained cellulose aerogel was tested by the transient plane heat source method, and the visible light transmittance and haze of the obtained cellulose aerogel were measured by GB / T2410-2008. The results showed that the thermal conductivity of the obtained cellulose aerogel was 0.0241 W / (m·K), the average visible light transmittance was 85.48%, and the haze was less than 12%.
[0087] Figure 1 This is a photo of the obtained cellulose aerogel.
[0088] Example 2
[0089] The difference from Example 1 is that S1 is prepared with a TEMPO oxidized cellulose aqueous dispersion having a mass concentration of 2%, and the rest is the same as Example 1.
[0090] The thermal conductivity, visible light transmittance and haze of the obtained cellulose aerogel were tested by the method of Example 1. The results showed that the thermal conductivity of the obtained cellulose aerogel was 0.0308 W / (m·K), the average visible light transmittance was 78.35%, and the haze was 20%.
[0091] The preparation method of TEMPO oxidized cellulose is the same as that in Example 1.
[0092] By comparing Example 1 and Example 2, it can be seen that the concentration of the TEMPO oxidized cellulose aqueous dispersion will affect the thermal conductivity, visible light transmittance and haze of the final cellulose aerogel.
[0093] Comparative Example 1
[0094] The difference from Example 1 is that S2 is not performed, and the rest is the same as Example 1.
[0095] The thermal conductivity, visible light transmittance and haze of the obtained cellulose aerogel were tested by the method of Example 1. The results showed that the thermal conductivity of the obtained cellulose aerogel was 0.0268 W / (m·K), the average visible light transmittance was 78.85%, and the haze was 50%.
[0096] Comparative Example 2
[0097] The difference from Example 1 is that in S2, the homogenization times are 4 times, and in S3, the centrifugation time is 2 minutes; the rest is the same as in Example 1.
[0098] The thermal conductivity, visible light transmittance and haze of the obtained cellulose aerogel were tested by the method of Example 1. The results showed that the thermal conductivity of the obtained cellulose aerogel was 0.0256 W / (m·K), the average visible light transmittance was 82.18%, the haze was 21%, and there were some macropores in the aerogel.
[0099] Comparative Example 3
[0100] A method for preparing cellulose aerogel comprises the following steps:
[0101] S1. Prepare TEMPO oxidized cellulose according to the method of Example 1, and then prepare a TEMPO oxidized cellulose aqueous dispersion with a mass concentration of 1%, mix thoroughly and refrigerate in an ice bath at 5°C.
[0102] S2. Place the prepared TEMPO oxidized cellulose aqueous dispersion in a high-pressure homogenizer for homogenization. The pressure is set to 200 MPa. The homogenization times are 4 times, and the homogenization time for each time is 30 minutes.
[0103] S3. Place the homogenized system into a centrifuge and centrifuge at 7800 rpm for 10 min to obtain a centrifuged system; pour the centrifuged system into a 10 mm custom mold.
[0104] S4. Spray 1 mol / L hydrochloric acid solution into the centrifugal system in the form of spray through an electric fogger to make the pH value of the centrifugal system <3, and then let it stand for 0.5 h to obtain an oriented fiber system; immerse the oriented fiber system in a 1 mol / L hydrochloric acid aqueous solution for 24 h to form a hydrogel.
[0105] S5. After washing away the excess acid on the surface of the hydrogel with deionized water, the hydrogel is first placed in an ethanol aqueous solution with a volume concentration of 50% for a first exchange for 12 hours, and then the hydrogel is immersed in ethanol for a second exchange, the number of the second exchange is 7 times, and the exchange time for each exchange is 12 hours; then the hydrogel is placed in a supercritical dryer for drying; wherein the drying includes sequentially performing a carbon dioxide intake stage, a carbon dioxide extraction stage, and a carbon dioxide exhaust stage; the parameters of the carbon dioxide intake flushing stage include: a temperature of 5°C, a carbon dioxide flow rate of 2nL / min, and a holding time of 5h; the parameters of the carbon dioxide extraction stage include: a pressure of 10MPa, a temperature of 40°C, and a holding time of 2h; the parameters of the carbon dioxide exhaust stage include: a temperature of 40°C, a carbon dioxide flow rate of 80mL / min, and a holding time of 10h, to obtain a cellulose aerogel.
[0106] The thermal conductivity, visible light transmittance and haze of the obtained cellulose aerogel were tested by the method of Example 1. The results showed that the thermal conductivity of the obtained cellulose aerogel was 0.0242 W / (m·K), the average visible light transmittance was 55%, and the haze was 87%.
[0107] Example 3
[0108] A method for preparing cellulose aerogel comprises the following steps:
[0109] S1. Prepare TEMPO oxidized cellulose according to the method of Example 1, and then prepare a TEMPO oxidized cellulose aqueous dispersion with a mass concentration of 1%, mix thoroughly and refrigerate in an ice bath at 5°C.
[0110] S2. Place the prepared TEMPO oxidized cellulose aqueous dispersion in a high-pressure homogenizer for homogenization. The pressure is set to 200 MPa. The homogenization times are 3 times, and the homogenization time for each time is 30 minutes.
[0111] S3. The homogenized system was placed in a centrifuge and centrifuged at 7800 rpm for 10 min to obtain a centrifuged system; the centrifuged system was then poured into a 4 mm custom mold.
[0112] S4. Spray 0.1 mol / L hydrochloric acid solution into the centrifugal system in the form of spray through an electric fogger to make the pH of the centrifugal system <3, and then let it stand for 0.5 h to obtain an oriented fiber system; immerse the oriented fiber system in a 0.05 mol / L hydrochloric acid aqueous solution for 24 h to form a hydrogel.
[0113] S5. After washing away the excess acid on the surface of the hydrogel with deionized water, the hydrogel is first placed in an ethanol aqueous solution with a volume concentration of 50% for a first exchange for 12 hours, and then the hydrogel is immersed in ethanol for a second exchange, the number of the second exchange is 7 times, and the time of each exchange is 12 hours; then the hydrogel is placed in a supercritical dryer for drying; wherein the drying includes sequentially performing a carbon dioxide intake stage, a carbon dioxide extraction stage and a carbon dioxide exhaust stage; the parameters of the carbon dioxide intake flushing stage include: the temperature is preferably 5°C, the flow rate of carbon dioxide is 2nL / min, and the holding time is 5h; the parameters of the carbon dioxide extraction stage include: the pressure is 10MPa, the temperature is 40°C, and the holding time is 2h; the parameters of the carbon dioxide exhaust stage include: the temperature is 40°C, the flow rate of carbon dioxide is 80mL / min, and the holding time is 10h, thereby obtaining cellulose aerogel.
[0114] The thermal conductivity, visible light transmittance and haze of the obtained cellulose aerogel were tested by the method of Example 1. The results showed that the thermal conductivity of the obtained cellulose aerogel was 0.0304 W / (m·K), the average visible light transmittance was 74.15%, and the haze was 33%.
[0115] Comparative Example 4
[0116] A method for preparing cellulose aerogel comprises the following steps:
[0117] S1. Prepare a 1% TEMPO oxidized cellulose aqueous dispersion, mix thoroughly and refrigerate in an ice bath at 5°C.
[0118] S2. Place the prepared TEMPO oxidized cellulose aqueous dispersion in a high-pressure homogenizer for homogenization. The pressure is set to 200 MPa. The homogenization times are 4 times, and each homogenization lasts 30 minutes.
[0119] S3. The homogenized system was placed in a centrifuge and centrifuged at 7800 rpm for 10 min to obtain a centrifuged system; the centrifuged system was then poured into a 4 mm custom mold.
[0120] S4. Spray 0.5 mol / L hydrochloric acid solution into the membrane centrifugal system in the customized mold through an electric fogger in the form of a spray, so that the pH value of the centrifugal system is less than 3, and then let it stand for 0.5 h to obtain an oriented fiber system; then immerse the oriented fiber system in a 0.1 mol / L hydrochloric acid aqueous solution for 24 h to form a hydrogel.
[0121] S5. After washing away the excess acid on the surface of the hydrogel with deionized water, the gel was placed in a freeze drying machine and frozen for 12 hours, and then vacuum dried for 48 hours to obtain cellulose aerogel.
[0122] The thermal conductivity, visible light transmittance, haze and specific surface area of the obtained cellulose aerogel were tested by the method of Example 1. The results showed that the thermal conductivity of the obtained cellulose aerogel was 0.0644 W / (m·K), the average visible light transmittance was 61.54%, the haze was 72%, and the pore size distribution of the aerogel was uneven.
[0123] Comparative Example 5
[0124] The difference from Example 1 is that the process of "spraying 0.5 mol / L hydrochloric acid solution into the centrifugal system through an electric fogger in the form of a spray to make the pH of the centrifugal system <3, and then standing for 0.5 h to obtain an oriented fiber system" in S4 is omitted, and the film-formed system is directly immersed in a 0.1 mol / L hydrochloric acid solution for 24 h to form a hydrogel.
[0125] The other operations are the same as those in Example 1.
[0126] The thermal conductivity, visible light transmittance, haze and specific surface area of the obtained cellulose aerogel were tested by the method of Example 1. The results showed that the thermal conductivity of the obtained cellulose aerogel was 0.0421 W / (m·K), the average visible light transmittance was 73.64%, and the haze was 33%.
[0127] Comparative Example 6
[0128] The difference from Example 1 is that S4 is omitted.
[0129] The other operations are the same as those in Example 1.
[0130] The thermal conductivity, visible light transmittance, haze and specific surface area of the obtained cellulose aerogel were tested by the method of Example 1. The results showed that the thermal conductivity of the obtained cellulose aerogel was 0.0804 W / (m·K), the average visible light transmittance was 55.15%, and the haze was 62%.
[0131] Comparative Example 7
[0132] The difference from Example 1 is that in S4, 0.5 mol / L hydrochloric acid solution is sprayed in by means of a spray pot.
[0133] The other operations are the same as those in Example 1.
[0134] The thermal conductivity, visible light transmittance, haze and specific surface area of the obtained cellulose aerogel were tested by the method of Example 1. The results showed that the thermal conductivity of the obtained cellulose aerogel was 0.0323 W / (m·K), the average visible light transmittance was 78.89%, and the haze was 22%.
[0135] From the comparison between Example 1 and Comparative Examples 1 to 3, it can be seen that the homogenization treatment, the centrifugal treatment and the concentration of the first hydrochloric acid solution will affect the aerogel skeleton structure and its uniformity, and ultimately affect its various performances; and by changing the thickness of the film formed by the centrifugal system, the transmittance and haze of the transparent fiber aerogel can be adjusted; by changing the concentration of the TEMPO oxidized cellulose aqueous dispersion, the thermal conductivity and light transmittance of the transparent fiber aerogel can be adjusted.
[0136] From the comparison between Comparative Example 4 and Examples 1 to 3, it can be seen that the drying methods used in the preparation of cellulose aerogels in the present application are different. The transparent aerogel prepared by freeze-drying has a very uneven internal pore structure and high haze due to the irregular growth of ice crystals during the freezing process; the transparent cellulose aerogel prepared by supercritical drying has a uniform internal structure, high light transmittance and low haze, and has good thermal insulation function.
[0137] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing cellulose aerogel, It is characterized in that The following steps are involved: Providing a TEMPO oxidized cellulose aqueous dispersion; The TEMPO oxidized cellulose aqueous dispersion is subjected to homogenization and centrifugation in sequence to obtain a centrifugal system; After the centrifugal system is formed into a membrane, the first hydrochloric acid solution is sprayed into the membrane, and then the membrane is allowed to stand to obtain an oriented fiber system; The oriented fiber system is immersed in a second hydrochloric acid solution to form a gel to obtain a hydrogel; The hydrogel is sequentially washed, solvent replaced and dried to obtain the cellulose aerogel.
2. The preparation method according to claim 1, It is characterized in that The method for preparing TEMPO oxidized cellulose in the TEMPO oxidized cellulose aqueous dispersion comprises the following steps: After mixing cellulose, 2,2,6,6-tetramethylpiperidin-1-oxyl free radical, sodium bromide and water, sodium hypochlorite is added, and then a first oxidation is performed under alkaline conditions to obtain a pre-oxidized cellulose dispersion; The pre-oxidized cellulose dispersion, 2,2,6,6-tetramethylpiperidin-1-oxyl free radical and sodium chlorite are mixed, and then sodium hypochlorite is added, and then a second oxidation is performed under acidic conditions to obtain the TEMPO oxidized cellulose.
3. The preparation method according to claim 2, It is characterized in that During the first oxidation process, the mass ratio of the cellulose, 2,2,6,6-tetramethylpiperidin-1-oxyl free radical and sodium bromide is 20:0.1-1:1-5; the amount ratio of the cellulose and sodium hypochlorite is 1 g:1-15 mmol; The alkaline pH value is 9 to 14; The temperature of the first oxidation is 10 to 65°C; After the first oxidation, dialysis is further performed to obtain the pre-oxidized cellulose dispersion and the dialysate respectively.
4. The preparation method according to claim 2, It is characterized in that During the second oxidation process, the mass ratio of the 2,2,6,6-tetramethylpiperidin-1-oxyl free radical, sodium chlorite and cellulose is 0.1-0.75:10-40:20; the dosage ratio of the sodium hypochlorite and cellulose is 10-200 mmol:20 g; The acidic pH value is 4 to 6.8; The temperature of the second oxidation is 10 to 65° C. and the time is 24 to 72 hours; After the second oxidation, dialysis is further performed, and the obtained dialysis dispersion is freeze-dried to obtain the TEMPO oxidized cellulose.
5. The preparation method according to any one of claims 1 to 4, It is characterized in that The mass concentration of the TEMPO oxidized cellulose aqueous dispersion is 0.5-3%.
6. The preparation method according to claim 1, It is characterized in that The pressure of the homogenization treatment is 50-200 MPa, the number of homogenization treatments is 1-4 times, and the time of each homogenization treatment is 10-60 minutes; The rotation speed of the centrifugal treatment is 6000-8000 rpm, and the time is 10 minutes.
7. The preparation method according to claim 1, It is characterized in that The concentration of the first hydrochloric acid solution is 0.1-1 mol / L, and after the first hydrochloric acid solution is sprayed, the pH of the resulting system is ≤3; The spraying method is atomization spray; The standing time is 15 to 60 minutes.
8. The preparation method according to claim 1, It is characterized in that The concentration of the second hydrochloric acid solution is 0.05 to 1 mol / L, the concentration ratio of the second hydrochloric acid solution to the first hydrochloric acid solution is 1:1 to 10, and the gelling time is 4 to 24 hours.
9. The preparation method according to claim 1, It is characterized in that The drying method is supercritical drying.
10. The cellulose aerogel prepared by the preparation method according to any one of claims 1 to 9, It is characterized in that The cellulose aerogel has a thermal conductivity of 0.01 to 0.04 W / (m·K), an average visible light transmittance of 70 to 90%, and a haze of 10 to 35%.