Metal aerogel composite material and preparation method thereof

By covering conductive or dielectric polymers on metal aerogels and filling in insulating flexible polymers, the physical destruction and stability of traditional probes during detection is solved, and metals with high compression stability and environmental stability are achieved. Aerogel composite material probe, suitable for component solder joint detection and performance testing.

CN119060540APending Publication Date: 2024-12-03HARBIN INSTITUTE OF TECHNOLOGY (SHENZHEN) (INSTITUTE OF SCIENCE AND TECHNOLOGY INNOVATION HARBIN INSTITUTE OF TECHNOLOGY SHENZHEN) +1
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411160898.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Traditional metal-based probes are prone to physical damage during component detection. The conductive glue-based probes are insufficient elasticity and have poor environmental stability, making it difficult to meet the application needs at high temperatures and humidity.

Method used

Using metal aerogel composite materials, the three-dimensional network structure of metal aerogel can be coated with conductive or dielectric polymers and can be filled with insulating flexible polymers to form materials with excellent elasticity and electrical properties, and are used to prepare lossless Soft probe.

Benefits of technology

It realizes high compression stability and strong environmental stability probes, can maintain conductive performance under high temperature and humidity conditions, and is suitable for solder joint detection and performance testing of components of various shapes and deformations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060540A_ABST
    Figure CN119060540A_ABST
Patent Text Reader

Abstract

The invention discloses a metal aerogel composite material and a preparation method thereof. The metal aerogel composite material comprises metal aerogel with a three-dimensional network structure and a conductive polymer or a dielectric polymer coated on the surface of the metal aerogel, and the metal aerogel composite material can also comprise an insulating flexible polymer filled in pores of the metal aerogel. The metal aerogel composite material disclosed by the invention has excellent elasticity, electrical properties and structural stability; the conductive polymer or the dielectric polymer is uniformly coated on the nano-scale metal aerogel with a three-dimensional network structure, so that the metal aerogel has excellent compression stability performance while meeting high conductivity, and the metal aerogel becomes an in-situ lossless soft probe with high compression stability performance; the device is widely applied to device welding spot detection and performance testing in electronic packaging. According to the invention, different insulating flexible polymers can be used to meet the application requirements of different flexibility and temperature, and the application range is wide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer composite materials, and in particular to a metal aerogel composite material and a preparation method thereof. Background Art

[0002] With the rapid development of the semiconductor industry, integrated circuits are gradually developing towards miniaturization, high density and high power, which has led to the solder joint detection and performance testing of small components becoming an urgent problem to be solved. Probe detection is a method of solder joint failure detection, which directly contacts the probe with the solder joint to achieve solder joint detection and performance testing of components.

[0003] At present, metal-based and conductive glue-based probes are mainly used for solder joint detection and performance testing of components. However, traditional metal-based probes are prone to physical damage to components and PCB boards during testing, such as surface scratches and defects; while conductive glue-based probes are made of high-filling precious metal-based conductive glue, which has limited elasticity, high requirements for supporting processing and dispensing equipment, and are expensive. They have poor high temperature and environmental stability and are prone to losing elasticity or aging and conductivity degradation under loads such as temperature and humidity. Therefore, in order to ensure the working performance and service life of components and PCB boards, it is of great significance to develop new probes. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a metal aerogel composite material and a preparation method thereof, aiming to solve the problems that traditional metal-based probes are prone to cause physical damage to components and PCB boards when testing components, and that conductive glue-based probes have insufficient elasticity and poor high temperature and environmental stability.

[0005] Metal aerogel is a porous material with a three-dimensional network structure, which has low density, good elasticity and flexibility, extremely high conductivity, and strong thermal-electro-chemical stability. Because it has a three-dimensional porous network structure, it provides the possibility of compounding with various high molecular polymers. Based on this, the present invention utilizes the special three-dimensional porous network structure of metal aerogel, adopts the skeleton formed by metal aerogel, and the conductive polymer or dielectric polymer coated on the surface of the metal aerogel, and can also include an insulating flexible polymer filled in the pores of the metal aerogel, so as to obtain a metal aerogel composite material by compounding. The preparation method is to first prepare the metal aerogel, then mix the metal aerogel with a conductive polymer monomer solution or a dielectric polymer monomer solution, and then fill or not fill with an insulating flexible polymer to obtain a metal aerogel composite material, and the obtained metal aerogel composite material has excellent elasticity, electrical properties and stability.

[0006] Specifically, the technical solution of the present invention is as follows:

[0007] A first aspect of the present invention provides a metal aerogel composite material, comprising:

[0008] A metal aerogel having a three-dimensional network structure.

[0009] A conductive polymer or a dielectric polymer coated on the surface of the metal aerogel.

[0010] Optionally, the metal aerogel composite material further includes: an insulating flexible polymer filled in the pores of the metal aerogel.

[0011] Optionally, the material of the metal aerogel is metal nanowires, and the metal nanowires are selected from one or more of silver nanowires, copper nanowires, nickel nanowires, gold nanowires and tin nanowires.

[0012] In the metal aerogel, the diameter of the metal nanowires is 30nm-1000nm, the gap size between the metal nanowires is 40nm-100μm, and the density of the metal nanowires is 1mg / cm 3 -600mg / cm 3 .

[0013] Optionally, the conductive polymer is selected from one or more of polypyrrole, polyacetylene, polyphenylene, polyacene, polythiophene, polyaniline and polysulfide;

[0014] The dielectric polymer is selected from one or more of polyimide, biaxially oriented polypropylene, polytetrafluoroethylene, polyethyleneimine, polyphenylene sulfide, and polyphenylene sulfide modified products.

[0015] Optionally, the thickness ratio of the metal aerogel to the coated conductive polymer is 20:1-1:20; or, the thickness ratio of the metal aerogel to the coated dielectric polymer is 20:1-1:20.

[0016] Optionally, the insulating flexible polymer is selected from one or more of polydimethylsiloxane, epoxy resin, phenolic resin, polyurethane, polyimide, urea-formaldehyde resin and silicone resin.

[0017] Optionally, 40%-100% of the pores of the metal aerogel are filled with the insulating flexible polymer to form a porous or fully filled structure based on the metal nanowire network.

[0018] A second aspect of the present invention provides a method for preparing a metal aerogel composite material, comprising the following steps:

[0019] Providing metal aerogels;

[0020] The metal aerogel is mixed with a conductive polymer monomer solution or a dielectric polymer monomer solution for a first predetermined time to form a conductive polymer or a dielectric polymer on the surface of the metal aerogel to obtain the metal aerogel composite material.

[0021] Optionally, after the conductive polymer or dielectric polymer is formed on the surface of the metal aerogel, the method further comprises mixing with an insulating flexible polymer solution for a second predetermined time to fill the pores of the metal aerogel with the insulating flexible polymer to obtain the metal aerogel composite material.

[0022] Optionally, the step of mixing the metal aerogel with a conductive polymer monomer solution or a dielectric polymer monomer solution for a first predetermined time to form a conductive polymer or a dielectric polymer on the surface of the metal aerogel to obtain the metal aerogel composite material specifically includes:

[0023] Providing a conductive polymer monomer solution, wherein the conductive polymer monomer solution comprises a conductive polymer monomer, an oxidant and a solvent;

[0024] Completely immersing the metal aerogel in a conductive polymer monomer solution for a first predetermined time to form a conductive polymer on the surface of the metal aerogel, and then washing and drying to obtain the metal aerogel composite material, wherein the first predetermined time is 1 hour to 48 hours;

[0025] Alternatively, providing a dielectric polymer monomer solution, the dielectric polymer monomer solution comprising a dielectric polymer monomer and a solvent;

[0026] The metal aerogel is completely immersed in a dielectric polymer monomer solution, reacted under heating conditions for a first predetermined time to form a dielectric polymer on the surface of the metal aerogel, and then cleaned and dried to obtain the metal aerogel composite material, wherein the heating temperature is 200-250°C and the first predetermined time is 0.1h-4h.

[0027] Beneficial effects: The metal aerogel composite material of the present invention has at least the following advantages:

[0028] First, the metal aerogel composite material of the present invention has excellent elasticity, electrical properties and environmental stability. The metal aerogel in the metal aerogel composite material has a three-dimensional network structure, which can maintain the three-dimensional network structure without collapse when compressed, twisted and bent, and there will be no conductive network disconnection, and the elasticity is excellent; and the conductive polymer or dielectric polymer can be evenly coated on the three-dimensional network structure of the metal aerogel, while meeting the high conductivity, it also has excellent compression stability. The conductivity of the metal aerogel composite material under compression can reach 10 6 -10 7S / m, which is far superior to traditional conductive adhesive materials, can be compressed by more than 90%, and can better adapt to various shapes and deformations.

[0029] Second, the metal aerogel composite material of the present invention uses a metal aerogel with an internal porosity of more than 99% as a matrix. The ultra-large porosity can be used to fill insulating flexible polymers. Different insulating flexible polymers can be used to meet application requirements of different flexibility and temperature, and have a wide range of applications. For example, polydimethylsiloxane can be used in scenes below 200°C, with high stability and transparency; silica gel can be used in scenes below 300°C; polyimide can be used in scenes above 300°C.

[0030] Third, the metal aerogel composite material of the present invention has strong environmental stability, self-hydrophobicity, acid and alkali resistance, etc., and can be quickly patterned to form the required probe array for completing device solder joint detection and customized testing of device performance in electronic packaging. Specifically, according to the solder joint distribution map, the metal aerogel composite material can be arrayed by laser processing to form probes of various sizes above 10μm, such as large-area probes for power devices and fixed impedance fine-pitch probes for chips (using dielectric polymer coating), so as to better cope with different application scenarios, and laser array processing can maintain extremely high processing accuracy. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a top view schematic diagram of the in-situ soft probe based on the metal aerogel composite material in Example 1.

[0032] Figure 2 This is a SEM image of the silver nanowire network uniformly coated with polypyrrole in Example 1.

[0033] Figure 3 This is a schematic diagram of the process for preparing an in-situ soft probe based on a metal aerogel composite material in Example 2. DETAILED DESCRIPTION

[0034] The present invention provides a metal aerogel composite material and a preparation method thereof. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0035] According to one embodiment of the present invention, there is provided a metal aerogel composite material, comprising:

[0036] A metal aerogel having a three-dimensional network structure.

[0037] A conductive polymer or a dielectric polymer coated on the surface of the metal aerogel.

[0038] In the embodiments of the present invention, the metal aerogel composite material has good elasticity, electrical properties and structural stability. The metal aerogel has an adjustable three-dimensional nano-network structure, and the conductive polymer or dielectric polymer can be evenly coated on the three-dimensional network structure at the nanoscale. While meeting the high conductivity, it also has excellent compression stability, making it an in-situ non-destructive soft probe with high compression stability, which is widely used in device solder joint detection and performance testing in electronic packaging. The preparation method of the metal aerogel composite material is simple and has good repeatability.

[0039] According to one embodiment of the present invention, the material of the metal aerogel is metal nanowires, that is, a metal aerogel having a three-dimensional network structure formed by cross-linking metal nanowires. The solid phase size and pore size of the metal aerogel are both in the nanometer order.

[0040] According to one embodiment of the present invention, the metal nanowires are selected from one or more of silver nanowires, copper nanowires, nickel nanowires, gold nanowires and tin nanowires.

[0041] In a preferred embodiment, the metal nanowires are silver nanowires.

[0042] According to one embodiment of the present invention, the diameter of the metal nanowire is 30nm-1000nm (such as 30nm, 50nm, 60nm, 80nm, 100nm, 300nm, 400nm, 600nm, 900nm, 1000nm, etc.), the gap size between the metal nanowires is 40nm-100μm (such as 40nm, 50nm, 60nm, 80nm, 100nm, 300nm, 400nm, 600nm, 900nm, 1μm, 10μm, 30μm, 50μm, 60μm, 80μm, 100μm, etc.), and the density of the metal nanowire is 1mg / cm 3 -600mg / cm 3 (e.g. 1mg / cm 3 、10mg / cm 3 、50mg / cm 3 、100mg / cm 3 、200mg / cm 3 、300mg / cm 3 , 400mg / cm 3 , 500mg / cm 3 、550mg / cm 3 、600mg / cm 3As well as specific point values ​​between the above point values, due to space limitations and for the sake of brevity, the present invention will no longer exhaustively list the specific point values ​​included in the range.

[0043] According to one embodiment of the present invention, the conductive polymer is selected from one or more of polypyrrole, polyacetylene, polyphenylene, polyacene, polythiophene, polyaniline and polysulfide. The conductive polymer can be greatly compressed and has excellent conductive properties and resilience.

[0044] In a preferred embodiment, the conductive polymer is polypyrrole, which can be compressed to a greater extent, has better conductivity, and can withstand more than 50,000 times of resilience.

[0045] According to one embodiment of the present invention, the dielectric polymer is selected from one or more of polyimide, biaxially oriented polypropylene, polytetrafluoroethylene, polyethyleneimine, polyphenylene sulfide, and polyphenylene sulfide modified products. When the compression resistance needs to remain unchanged, the dielectric polymer is selected to coat the metal aerogel. The above dielectric polymer can be greatly compressed and has excellent resilience.

[0046] According to one embodiment of the present invention, the ratio of the diameter of the metal nanowire to the thickness of the coated conductive polymer is 20:1-1:20, such as 1:20, 1:10, 1:1, 2:1, 3:1, 4:1, 6:1, 10:1, 15:1, 18:1, 20:1, etc.; or, the ratio of the diameter of the metal nanowire to the thickness of the coated dielectric polymer is 20:1-1:20, such as 1:20, 1:10, 1:1, 2:1, 3:1, 4:1, 6:1, 10:1, 15:1, 18:1, 20:1, etc.

[0047] According to an embodiment of the present invention, the insulating flexible polymer is selected from one or more of polydimethylsiloxane, epoxy resin, phenolic resin, polyurethane, polyimide, urea-formaldehyde resin and silicone resin.

[0048] In the embodiments of the present invention, different insulating flexible polymers can be used to meet application requirements of different flexibility and temperature. For example, polydimethylsiloxane can be used in scenarios below 200°C, with high stability and transparency; silicone can be used in scenarios below 300°C; and polyimide can be used in scenarios above 300°C.

[0049] In a preferred embodiment, the insulating flexible polymer is polydimethylsiloxane, because the material has good stability and elasticity.

[0050] According to one embodiment of the present invention, 40%-100% (such as 40%, 50%, 60%, 70%, 80%, 90%, 100%, etc.) of the pores of the metal aerogel are filled with the insulating flexible polymer to form a porous or fully filled structure based on a metal nanowire network.

[0051] According to one embodiment of the present invention, a method for preparing a metal aerogel composite material is provided, which comprises the following steps:

[0052] S1. providing metal aerogel;

[0053] S2. Mixing the metal aerogel with a conductive polymer monomer solution or a dielectric polymer monomer solution for a first predetermined time to form a conductive polymer or a dielectric polymer on the surface of the metal aerogel to obtain the metal aerogel composite material.

[0054] According to one embodiment of the present invention, the method for preparing the metal aerogel composite material further comprises the steps of:

[0055] S3, after the conductive polymer or dielectric polymer is formed on the surface of the metal aerogel, mixing with the insulating flexible polymer solution for a second predetermined time to fill the pores of the metal aerogel with the insulating flexible polymer to obtain the metal aerogel composite material.

[0056] In an embodiment of the present invention, when a conductive polymer is formed on the surface of the metal aerogel, the preparation method comprises: preparing the metal aerogel; mixing a diluted low-solubility conductive polymer monomer solution with the metal aerogel, using an oxidant such as silver nitrate to release Ag; + The oxidizability of the metal aerogel and the self-adsorption effect of the reaction products on the metal nanowires such as nanosilver wires during the oxidation reaction form a conductive polymer by in-situ growth on the surface of the metal aerogel; then it is mixed with the insulating flexible polymer solution, and the metal aerogel composite material is obtained by toughening and curing the insulating flexible polymer. The metal aerogel composite material has good elasticity, electrical properties and structural stability. The preparation method of the metal aerogel composite material is simple, repeatable, mature and reliable, and has low environmental requirements. It is expected to solve the current problems of solder joint detection and performance testing of small components. At the same time, the metal aerogel composite material has obvious application advantages compared with traditional conductive adhesive materials.

[0057] In an embodiment of the present invention, when a dielectric polymer is formed on the surface of the metal aerogel, the preparation method includes: preparing a metal aerogel; mixing a diluted low-solubility dielectric polymer monomer solution with the metal aerogel, and forming a dielectric polymer by in-situ growth of the dielectric polymer monomer on the surface of the metal aerogel at 200-250°C (such as 220°C); and then mixing with an insulating flexible polymer solution, and toughening and curing the insulating flexible polymer to obtain the metal aerogel composite material. The metal aerogel composite material has good elasticity, electrical properties and structural stability. The preparation method of the metal aerogel composite material is simple, repeatable, mature and reliable, and has low environmental requirements, and is expected to solve the current problems of solder joint detection and performance testing of small components. At the same time, the metal aerogel composite material has obvious application advantages compared to traditional conductive adhesive materials.

[0058] In step S1, in one embodiment, the metal aerogel is prepared by the following method: preparing a metal hydrogel skeleton by liquid phase induced reduction method, washing and drying the metal hydrogel skeleton to obtain the metal aerogel. The metal aerogel can be cut into a specified size according to the actual drawing size.

[0059] In one embodiment, the reducing agent used in the liquid phase induced reduction method is ethylene glycol, the reaction temperature is 120° C.-150° C., and the reaction time is 3 h-5 h.

[0060] In one embodiment, the drying method is freeze drying or supercritical drying; preferably supercritical drying.

[0061] In one embodiment, the drying time is 3h-10h.

[0062] The preparation method of metal aerogel is prior art and will not be described in detail here.

[0063] In step S2, in one embodiment, the metal aerogel is mixed with a conductive polymer monomer solution for a first predetermined time to form a conductive polymer on the surface of the metal aerogel. The step of obtaining the metal aerogel composite material specifically includes:

[0064] Providing a conductive polymer monomer solution, wherein the conductive polymer monomer solution comprises a conductive polymer monomer, an oxidant and a solvent;

[0065] The metal aerogel is completely immersed in a conductive polymer monomer solution for a first predetermined time to form a conductive polymer on the surface of the metal aerogel, and then washed and dried to obtain the metal aerogel composite material, wherein the first predetermined time is 1h-48h, such as 1h, 5h, 10h, 13h, 15h, 20h, 25h, 30h, 33h, 35h, 40h, 45h, 48h, etc. As well as specific point values ​​between the above point values, the present invention no longer exhaustively lists the specific point values ​​included in the range due to space limitations and for simplicity.

[0066] In one embodiment, the conductive polymer monomer solution comprises a conductive polymer monomer, an oxidant and a solvent (such as a mixed solution of water and ethanol, etc.). Preferably, the oxidant is silver nitrate. Preferably, the conductive polymer monomer is selected from one or more of pyrrole, acetylene, phenylene, acene, thiophene, aniline and thioether.

[0067] Preferably, in the conductive polymer monomer solution, the concentration of the conductive polymer monomer is 0.1 μM-1M (such as 0.1 μM, 0.5 μM, 1 μM, 2 μM, 3 μM, 10 μM, 20 μM, 50 μM, 80 μM, 100 μM, 500 μM, 800 μM, 1M, etc.), and the concentration of the oxidant is 0.1 μM-1M (such as 0.1 μM, 0.5 μM, 1 μM, 2 μM, 3 μM, 10 μM, 20 μM, 50 μM, 80 μM, 100 μM, 500 μM, 800 μM, 1M, etc.). The use of low concentrations of conductive polymer monomers and oxidants can make the reaction slow and uniform, thereby ensuring that a conductive polymer coating layer with uniform thickness is formed on the surface of the metal aerogel.

[0068] In one embodiment, the step of mixing the metal aerogel with a dielectric polymer monomer solution for a first predetermined time to form a dielectric polymer on the surface of the metal aerogel to obtain the metal aerogel composite material specifically includes:

[0069] providing a dielectric polymer monomer solution, the dielectric polymer monomer solution comprising a dielectric polymer monomer and a solvent;

[0070] The metal aerogel is completely immersed in a dielectric polymer monomer solution, reacted under heating conditions for a first predetermined time to form a dielectric polymer on the surface of the metal aerogel, and then washed and dried to obtain the metal aerogel composite material, wherein the heating temperature is 200-250°C (such as 220°C), and the first predetermined time is 0.1h-4h, such as 0.1h, 0.5h, 1h, 2h, 3h, 4h, etc. As well as specific point values ​​between the above point values, the present invention no longer exhaustively lists the specific point values ​​included in the range due to space limitations and for simplicity.

[0071] In one embodiment, the dielectric polymer monomer solution includes a dielectric polymer monomer and a solvent; preferably, the dielectric polymer monomer is selected from one or more corresponding monomers such as polyimide, biaxially oriented polypropylene, polytetrafluoroethylene, polyethyleneimine, polyphenylene sulfide, and polyphenylene sulfide modifications.

[0072] Preferably, in the dielectric polymer monomer solution, the volume concentration of the dielectric polymer monomer is 0.1-10%, such as 0.1%, 0.5%, 1%, 5%, 10%, etc. As well as specific point values ​​between the above point values, the present invention no longer exhaustively lists the specific point values ​​included in the above range due to space limitations and for the sake of simplicity. The use of low concentrations of dielectric polymer monomers can make the reaction slow and uniform, thereby ensuring that a dielectric polymer coating layer of uniform thickness is formed on the surface of the metal aerogel.

[0073] In one embodiment, the drying method is freeze drying or supercritical drying; preferably supercritical drying.

[0074] In one embodiment, the drying time is 0.5h-3h, such as 0.5h, 1h, 1.2h, 1.5h, 1.9h, 2.3h, 2.6h or 3h. As well as specific values ​​between the above values, due to space limitations and for the sake of simplicity, the present invention will no longer exhaustively list the specific values ​​included in the range.

[0075] In one embodiment, step S3 specifically includes: after a conductive polymer or a dielectric polymer is formed on the surface of the metal aerogel, completely immersing it in an insulating flexible polymer solution for a second predetermined time, wherein the second predetermined time is 30s-8h (such as 30s, 60s, 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, etc.), and then filtering and curing to obtain the metal aerogel composite material.

[0076] In one embodiment, the insulating flexible polymer solution includes an insulating flexible polymer and a curing agent.

[0077] In one embodiment, the curing agent is selected from one or more commonly used cross-linking agents, end-capping agents, and the like.

[0078] In one embodiment, the filtration temperature is 30°C-50°C, for example, 30°C, 35°C, 40°C, 45°C or 50°C, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0079] In one embodiment, the filtration method is vacuum filtration.

[0080] In one embodiment, the vacuum filtration time is 0.5h-4h, for example 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h or 4h, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0081] In one embodiment, the curing method is heat curing.

[0082] In one embodiment, the heating and curing temperature is 60°C-100°C, for example 60°C, 70°C, 80°C, 90°C or 100°C, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0083] In one embodiment, the heating curing time is 0.5h-7h, for example 0.5h, 1.5h, 3.0h, 5.5h or 7.0h, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0084] In another embodiment, step S3 specifically includes: after a conductive polymer or a dielectric polymer is formed on the surface of the metal aerogel, compounding it with an insulating flexible polymer solution by a percolation compounding method, placing it in a vacuum box for low-pressure degassing, and then placing it on a heating platform for heating and curing to obtain the metal aerogel composite material.

[0085] In one embodiment, the insulating flexible polymer solution includes an insulating flexible polymer and a curing agent.

[0086] In one embodiment, the curing agent is selected from one or more commonly used cross-linking agents, end-capping agents, and the like.

[0087] In one embodiment, the low-pressure degassing time is 5-15 min, such as 10 min.

[0088] In one embodiment, the heating and curing temperature is 60°C-100°C, for example 60°C, 70°C, 80°C, 90°C or 100°C, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0089] In one embodiment, the heating curing time is 0.5h-7h, for example 0.5h, 1.5h, 3.0h, 5.5h or 7.0h, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0090] According to one embodiment of the present invention, there is provided an application of a metal aerogel composite material in detecting solder joints of devices in electronic packaging.

[0091] According to one embodiment of the present invention, there is provided an application of a metal aerogel composite material in device performance testing in electronic packaging.

[0092] The present invention will be further described below by means of specific examples.

[0093] Example 1

[0094] A method for preparing an in-situ nondestructive soft probe based on a metal aerogel composite material, the specific method comprising:

[0095] (1) Preparation of 0.1 M AgNO 3 The precursor aqueous solution was sequentially added with 0.12M citric acid reducing agent, 0.03M polyvinyl pyrrolidone surfactant and catalyst, and reacted at 150°C for 6h to induce liquid phase reduction reaction to prepare silver nanowire hydrogel, and the silver nanowire hydrogel was dried into silver nanowire aerogel by supercritical drying method, and the silver nanowire aerogel was cut and compressed by laser beam and hydraulic method to obtain layered silver nanowire aerogel with a thickness of 5mm;

[0096] (2) compressing a 5 mm thick silver nanowire aerogel into a 2 mm thick silver nanowire aerogel, and then immersing it in a mixed solution containing 2 μM pyrrole, 3 μM silver nitrate, 15 mL water and 15 mL ethanol for 24 h, and drying it for 1 h by supercritical drying to obtain a polypyrrole-coated metal aerogel;

[0097] (3) Using a thin layer of silver glue, the polypyrrole-coated metal aerogel obtained in step (2) is mounted on the target pad array, and the polypyrrole-coated metal aerogel is array-processed by pulsed laser to obtain a polypyrrole-coated metal aerogel array that is conformal and stably connected to the pad array, wherein the laser power is selected to be 2 W and the laser processing speed is selected to be 100 mm / s; then, polydimethylsiloxane and a curing agent are mixed in a volume ratio of 10:1, placed in a vacuum box for low-pressure degassing for 2 minutes, and allowed to stand for 15 minutes to obtain a polydimethylsiloxane solution, and then 21g of polydimethylsiloxane is compounded with the polypyrrole-coated metal aerogel array structure by a percolation composite method, and placed in a vacuum box for low-pressure degassing for 10 minutes, and then placed on a heating platform for heating and curing, the curing temperature is 80°C, and the curing time is 0.5h, so that an in-situ non-destructive soft probe based on a metal aerogel composite material can be obtained. Figure 1 .

[0098] After testing, the conductivity of the polypyrrole-coated metal aerogel obtained in step (2) of this embodiment can reach 20000 S / m. The SEM image of the polypyrrole-coated metal aerogel is shown in FIG. Figure 2 Due to the low concentration of pyrrole and oxidant, the reaction is slow and uniform, and a polypyrrole coating layer with uniform thickness can be formed on the surface of the metal aerogel. The polypyrrole-coated metal aerogel has a low modulus and stable compression performance, and the interior can be well filled with polydimethylsiloxane.

[0099] The conductivity of the in-situ nondestructive soft probe based on the metal aerogel composite material obtained in step (3) can reach 10,000 to 30,000 S / m, and the diameter of a single probe can reach 10 microns. The compression amount of the soft probe can reach 80%, and the number of compressions can exceed 100,000 times, which can be applied to the performance testing of devices and chips of various sizes.

[0100] Example 2

[0101] A method for preparing an in-situ nondestructive soft probe based on a metal aerogel composite material, such as Figure 3 As shown ( Figure 3 In the figure, 1 is a PVA sacrificial layer, 2 is a silicon wafer, 3 is a layered polyimide-coated metal aerogel, 4 is a polyimide-coated metal aerogel array, 5 is silica gel, and 6 is an in-situ nondestructive soft probe based on a metal aerogel composite material), and the specific method includes:

[0102] (1) Preparation of 0.1 M AgNO 3 The precursor aqueous solution was sequentially added with 0.12M citric acid reducing agent, 0.03M polyvinyl pyrrolidone surfactant and catalyst, and reacted at 150°C for 6h to induce liquid phase reduction reaction to prepare silver nanowire hydrogel, and the silver nanowire hydrogel was dried into silver nanowire aerogel by supercritical drying method, and the silver nanowire aerogel was cut and compressed by laser beam and hydraulic method to obtain layered silver nanowire aerogel with a thickness of 10mm;

[0103] (2) compressing a 10 mm thick silver nanowire aerogel into a 1 mm thick silver nanowire aerogel, immersing it in 30 mL of a 2 vol.% polyimide monomer solution, heating it to 220° C. for 2 h, and drying it for 2 h by supercritical drying to obtain a polyimide-coated metal aerogel;

[0104] (3) Spin-coating a 30 μm thick PVA sacrificial layer on a silicon wafer, placing the polyimide-coated metal aerogel obtained in step (2) on the surface of the sacrificial layer, gently pressing it into the sacrificial layer, and heating at 80° C. for 30 min to complete curing;

[0105] (4) processing the polyimide-coated metal aerogel array by pulse laser, wherein the laser power is 0.8 W and the laser processing speed is 50 mm / s, to obtain a polyimide-coated metal aerogel array located on the sacrificial layer;

[0106] (5) Silica gel and curing agent were mixed in a volume ratio of 10:1, placed in a vacuum box for low-pressure degassing for 2 minutes, and allowed to stand for 15 minutes to obtain a silica gel solution. The obtained solution was filled in and between the polyimide-coated metal aerogel arrays, with the liquid level lower than the top surface of the polyimide-coated metal aerogel array. After sufficient standing and degassing treatment, the solution was heated at 80°C for 30 minutes to complete the curing of the polymer. The obtained structure was then immersed in desorption solvent water to dissolve the sacrificial layer, thereby obtaining an in-situ non-destructive soft probe based on the metal aerogel composite material.

[0107] Compared with Example 1, the soft probe of this embodiment is an independent device and can be replaced according to the needs of use. After being filled with silicone, the strength and toughness of the soft probe are greatly improved. It can withstand pressure above 150PSI and rebound spontaneously, but the compressibility is reduced to only about 50%.

[0108] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A metal aerogel composite material, characterized in that: include: A metal aerogel having a three-dimensional network structure. A conductive polymer or a dielectric polymer coated on the surface of the metal aerogel.

2. The metal aerogel composite material according to claim 1, characterized in that: The metal aerogel composite material further includes: an insulating flexible polymer filled in the pores of the metal aerogel.

3. The metal aerogel composite material according to claim 1, characterized in that: The material of the metal aerogel is metal nanowires, and the metal nanowires are selected from one or more of silver nanowires, copper nanowires, nickel nanowires, gold nanowires and tin nanowires. In the metal aerogel, the diameter of the metal nanowires is 30nm-1000nm, the gap size between the metal nanowires is 40nm-100μm, and the density of the metal nanowires is 1mg / cm 3 -600mg / cm 3 .

4. The metal aerogel composite material according to claim 1, characterized in that: The conductive polymer is selected from one or more of polypyrrole, polyacetylene, polyphenylene, polyacene, polythiophene, polyaniline and polysulfide; The dielectric polymer is selected from one or more of polyimide, biaxially oriented polypropylene, polytetrafluoroethylene, polyethyleneimine, polyphenylene sulfide, and polyphenylene sulfide modified products.

5. The metal aerogel composite material according to claim 1, characterized in that: The thickness ratio of the metal aerogel to the coated conductive polymer is 20:1-1:20; or, the thickness ratio of the metal aerogel to the coated dielectric polymer is 20:1-1:

20.

6. The metal aerogel composite material according to claim 2, characterized in that: The insulating flexible polymer is selected from one or more of polydimethylsiloxane, epoxy resin, phenolic resin, polyurethane, polyimide, urea-formaldehyde resin and silicone resin.

7. The metal aerogel composite material according to claim 2, characterized in that: 40%-100% of the pores of the metal aerogel are filled with the insulating flexible polymer.

8. A method for preparing the metal aerogel composite material according to any one of claims 1 to 7, characterized in that: The following steps are involved: Providing metal aerogels; The metal aerogel is mixed with a conductive polymer monomer solution or a dielectric polymer monomer solution for a first predetermined time to form a conductive polymer or a dielectric polymer on the surface of the metal aerogel to obtain the metal aerogel composite material.

9. The preparation method according to claim 8, characterized in that: After the conductive polymer or dielectric polymer is formed on the surface of the metal aerogel, the method further comprises mixing with an insulating flexible polymer solution for a second predetermined time to fill the pores of the metal aerogel with the insulating flexible polymer to obtain the metal aerogel composite material.

10. The preparation method according to claim 8, characterized in that: The step of mixing the metal aerogel with a conductive polymer monomer solution or a dielectric polymer monomer solution for a first predetermined time to form a conductive polymer or a dielectric polymer on the surface of the metal aerogel to obtain the metal aerogel composite material specifically includes: Providing a conductive polymer monomer solution, wherein the conductive polymer monomer solution comprises a conductive polymer monomer, an oxidant and a solvent; Completely immersing the metal aerogel in the conductive polymer monomer solution for a first predetermined time to form a conductive polymer on the surface of the metal aerogel, and then washing and drying to obtain the metal aerogel composite material, wherein the first predetermined time is 1 hour to 48 hours; Alternatively, providing a dielectric polymer monomer solution, the dielectric polymer monomer solution comprising a dielectric polymer monomer and a solvent; The metal aerogel is completely immersed in a dielectric polymer monomer solution, reacted under heating conditions for a first predetermined time to form a dielectric polymer on the surface of the metal aerogel, and then cleaned and dried to obtain the metal aerogel composite material, wherein the heating temperature is 200-250°C and the first predetermined time is 0.1h-4h.

Citation Information

Cited By

  • Self-rebounding tubular composite heat-conducting pad based on metal aerogel and preparation method and application of self-rebounding tubular composite heat-conducting pad

    CN119570461A

  • Self-rebound tubular composite thermal pad based on metal aerogel, its preparation method and application

    CN119570461B

  • Multilayer flexible circuit, preparation method thereof and flexible electronic system

    CN121057097A

  • Multilayer flexible circuit and method of making same, flexible electronic system

    CN121057097B